MISRI, BASED ON MY EXPERIENCE, YOU CAN USE 5:1 ETCH. 5 PARTS FUMING NITRIC ACID AND 1 PART CONCENTRATED SULFURIC ACID. ------------ NOTE, I UNDERLINE CONCENTRATED TO EMPHASIZE THIS TYPE AND NOT FUMING SULFURIC ACID. MIXING BOTH FUMING HNO3 AND H2SO4 CAN CAUSE SEVERE EXPLOSION. TO BE SAFE, WHEN YOU DECAP, DECAP ALSO CONTROLLED STRIPS W/ KNOWN SILVER TO BE ON THE STRIPS. HEAT UP THE ACID ON HOT PLATE, LET IT BOILS AND DIP THE UNITS/ STRIPS FOR 1-2 MINUTES TILL MOLD DISAPPEARS. BR, NIK X1614 I'm using Copper Lead frame (plated copper over Alloy 42) and Silver strip layer for die and wire bonding area. This is for SOT 23/ SC 59 packages. We just notice that the incomming leadframe is having intermittant 'missing silver' problem. Unfortunately about 20K products have been molded (incapsulated). Now i want to Decapsulate (remove the mold compound) some sample to identify how serious the problem is. What chemical/solution is best to do this work. The solution should NOT attack the Copper and silver layer. Thus I can identify the missing silver area products. Fuming Nitric Acid?, Fuming Sulfuric acid?, Mix 50-50 ? Appreciate yr inputs. Regards Mohd Misri Seremban BIM *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To subscribe/unsubscribe send a message <to: [log in to unmask]> * * with <subject: subscribe/unsubscribe> and no text in the body. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************