In a message dated 97-06-09 11:39:36 EDT, you write: << Our customer's product is to be used in aeroplane. It has lot of Leadless Chip Carrier (LCC) package IC. The LCC's solder joint cracked during the FCC vibration and thermal test. Could anyone have experience with similiar problem share it with me? We are currently looking looking into 2 different solutions: 1. PCB finish plating and solder paste. 2. Converting LCC to leaded package. Other suggestions are deeply appeciated >> Steve, The problem is solder fatigue and is driven by cyclic stress and strains caused by thermal expansion mismatch between the board and the component. This is a common problem with LCCCs on substrates that have a large in-plane Coefficient of Thermal Expansion (CTE). Ways to reduce the incidence of solder joint fatigue include: a. use a substrate that is better CTE-matched to the LCCC b. increase the component stand-off height c. if the LCCC is a castellated device, increase solder volume to increase the fillet size (larger fillets provide for lower stress, and it takes longer to propagate fatigue cracks thru a large size fillet). Upfront reliability modeling should tell you how much gain you can expect in solder joint life from each of the above. d. switch to a leaded package with leads that are compliant enough. Depending on component size and expected thermal cycles in use, "a, b or c" may not be enough and switching to a leaded package may be the only way to go. With best regards, Jean-Paul ________________________________________________________________ Jean-Paul Clech EPSI Inc., P. O. Box 1522, Montclair, NJ 07042 - USA tel: +1 (201)746-3796 fax: + 1 (201)655-0815 Home page: <A HREF="http://members.aol.com/Epsiinc1/index.html">http://members.aol.com/Ep siinc1/index.html</A> (last updated on May June 9, 1997). - click on the above or copy: http://members.aol.com/Epsiinc1/index.html __________________________________________________________________ Note: as of June 1, 1997, our area code will change from 201 to 973. From June 1st until December 6th, 1997, both 973 and 201 area codes will work. *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To subscribe/unsubscribe send a message <to: [log in to unmask]> * * with <subject: subscribe/unsubscribe> and no text in the body. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************