Peter, I would agree with Karen Tellefsen. In the past 6 months or so, we have seen four or five problem cases where the culprit was a latex peelable solder mask. The data that Karen provided is similar to what I have seen with SIR data, probably even lower. Part of the problem is the material itself (ammonia based are worse), which often leaves behind either halides or a conductive organic residue. In the former, you get corrosion and metal migration. In the latter you get electrical leakage. The situation is worse for no-clean assemblers since there is no opportunity to remove the residues. As Karen said, no visible residue does not mean no residue. Another fault mechanism we have seen is that the materials can outgas during thermal exposures, contaminating regions around the latex mask. Often, conformal coating will not stick to the latex mask residues. I don't agree with your supposition that thousands of companies are using it with no problems. Lots of companies have intermittent problems they can't explain or believe their local rep "there's absolutely no problems with my product, buy 10 cases". This is becoming a much bigger issue as more companies move out of the cleaning realm (or couldn't make no-clean work) and into no-clean technology. I may have a rather jaded view, but those four or five cases I mentioned earlier - all had been told that no visible residue means no residues and everything is AOK with the product. Must be something in your assembly process Bucko. Doug Pauls CSL *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To subscribe/unsubscribe send a message <to: [log in to unmask]> * * with <subject: subscribe/unsubscribe> and no text in the body. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************