This is a classic problem with "double sided cap construction". The outer cores are expanding and contracting at the CTE of your lamination plates and separator plates. Your internal cores are expanding and contracting at the CTE of their copper cladding. If you are stuck with using "double sided cap" construction, try using what are called a "clutch plate" inserts. When laying up your panel, first put down a sacrificial piece of foil, then a ply of 1080 pre-preg, then a piece of sacrificial foil (This creates the "clutch plate" effect), you then lay-up your panel directly on the "clutch plate", finishing with another "clutch plate" insert on the top of the panel stack. This will allow the two outer cores to move the same as the internal cores... It does add cost to the process, but it is difficult to scale or adjust the outer cores to the variables of expansion in your metal lamination plates... Good Luck, Scott Baller Engineering Manager MULTEK Roseville [log in to unmask] ______________________________ Reply Separator _________________________________ Subject: (Fwd) Re: FAB(Shifting Layers) Author: [log in to unmask] at INTERNET_GATEWAY Date: 3/21/97 6:19 AM Forwarded message: From: Self <Single-user mode> To: [log in to unmask] Subject: Re: FAB(Shifting Layers) Date: Fri, 21 Mar 1997 08:45:45 > We are experincing a reaccuring problem with our lamination process on 10 > layer projects with the following stackup: > > 1. 1 oz copper on all 5 FR4 5 mil sheets; > 2. 3 sheets of PGFK1080 2.5mil prepreg in each gap (total of 7.5mils each > gap); > 3. Grain of prepreg is in the same direction; > 4. finished thickness 69 mils; > 5. layers 2-4 & 7-9 are signal layers; > 6. layers 5&6 are ground/VCC planes. > > Problem: We are consistently seeing layers 2 and 9 shift 3-4 mils more than > the other layers (3:4, 5:6, & 7:8). Layers 3:4, 5:6, & 7:8 all align well > with each other and the outermost sheets are shifted to the right by this 3-4 > mils. Once layers 1 and 10 are imaged onto the drilled panel, they also line > up well with the innermost layers (3:4, 5:6, & 7:8). We are losing panels due > to annualar rings less than 2 mils on layers 2 & 9 (Mil-P-55110). > > We would appreciate any suggestions from those who have seen similar > occurances. > > Patty Causey / Marty W. Sheppard > Process Engineering Section > email address: [log in to unmask] / > [log in to unmask] > Phone: (912) 926-9473(9632) > There's a couple of things you can do to fix this problem. 1. Go to a foil construction if you can. The all core construction with solid copper on the outer layers tends to"lock in" the outer most cores, where the inner cores will shrink as expected, unconstricted. This is seen more with the use of aluminum seperator plates than with steel plates. 2. If all core is the only option, etch off all the copper on the outer layers and replace with foil and a single ply of prepreg at lamination. This prevents the "lock in" effect. In addition, 3 plys of the same glass style of prepreg should be avoided, especially a light glass like 1080. These tend to "swim" on each other during lamination. Try to stay with 2 plys, say 106, 2116 or 1080, 2313. Robert P. McGarry jr Technical Sales Analyst Proto Circuit Inc. 2035 Midway Dr. Twinsburg, OH. 44087 216-425-4939 fx. 216-425-9704 [log in to unmask] "QUALITY MANUFACTURED PRINTED CIRCUIT BOARDS" *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To subscribe/unsubscribe send a message <to: [log in to unmask]> * * with <subject: subscribe/unsubscribe> and no text in the body. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * *************************************************************************** *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To subscribe/unsubscribe send a message <to: [log in to unmask]> * * with <subject: subscribe/unsubscribe> and no text in the body. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************