Try cooling the boards more rapidly as they exit the solder wave. There is an excellent paper by Rockwell-Collins (Hagge and Mather were the authors) in the early China Lake Soldering Seminar Proceedings on problems with grainy-looking or "cold" solder joints from vapor phase soldering. They found that slow cooling allowed the grain structure to become quite coarse, which gave the "grainy" look. In the paper, they reported an accelerated cooling profile which gave reliable joints with the desired fine grain structure, which gave the desired look to meet cosmetic criteria. If running a scrap board through the machine and using a hair dryer to rapidly cool these large joints gives the desired look, then I think some pull strength tests would settle the issue. The paper was given at the '82 China Lake meeting, but only the abstract is in the proceedings. The paper was published elsewhere. --Bill Kenyon Global Centre for Process Change, Inc. 302-652-4272/-5701 Tel/Fax *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To subscribe/unsubscribe send a message <to: [log in to unmask]> * * with <subject: subscribe/unsubscribe> and no text in the body. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************