I am assuming that you are talking about aqueous processible LPI solder masks, so a few suggestions would be: 1. Bake the boards for 30-60 min at 250 deg F to really dry the boards. At this point the mask is very, very dry and is more impervious to absorbing moisture from aqueous processes (think in terms of a bone dry Chamois that is very difficult to wet out when it is dry, but absorbs water easily when it becomes damp) 2. Oxide processes tend to be highly alkaline (>13.0 pH) and operate at high temp (up to 160 deg F). Try to keep the exposure of the mask to a minimum in this type of environment. Aqueous LPI masks are developed is alkaline media and are much less resistant to alkaline solutions than to acidic ones (in fact, aqueous LPI masks can be stripped after they are cured in highly alkaline, high temperature solutions). High alkalinity, high temperatures and long exposure times are not your friends, so try to minimize all of these. It is possible that the aqueous LPI masks will never work well in your process. There may be other alternatives for masks: 1. One or two component thermal cure epoxy solder masks are highly impervious to both highly acid or alkaline solutions. The down side here is that the resolution capabilities of these masks are not as good as the LPI's. 2. There is a LPI solder mask from Ciba Geigy called Probimer 52. This mask is developed in a solvent (not aqueous) and is highly impervious to both highly acidic and alkaline solutions. Only about 20 shops in North America have this system installed (system costs >$500,000); however, there are several services in the USA that process Probimer 52 for PWB manufacturers. They are: A. Solder Station One Santa Ana, CA Mr. Odilon Cardenas B. Independent Technology Systems (ITS) Bloomington, MN Mr. Don Paterson C. Radian Technologies Austin, TX I hope this information helps. Please contact me if I can be of further service. Larry Fisher Dexter Electronic Materials [log in to unmask] *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To unsubscribe from this list at any time, send a message to: * * [log in to unmask] with <subject: unsubscribe> and no text. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************