Hi Steve - One possible explanation for your one solder pot to be low in tin is the amount of drossing and/or drossing conditions that it has seen since your last analysis. You will lose tin content from your solder pot as part of the de-drossing operations. Since solder is more tin than lead (ie. 63 tin - 37 lead) and tin preferentially oxidizes versus lead, its almost logical that your dross will impact your tin content to some level. Some testing results we gathered on our dross content (for another reason entirely than low tin) confirmed that this could be one contributor. You should probably check out what method of solder alloy analysis was used too - what is the typical measurement error for the analysis method and could it impact the number you are getting reported as a result. Then again if you were cooking potatoes or getting rid of solder paste on your solder pot then lots of strange interactions could happen!!!! Good Luck. Dave Hillman Rockwell Collins [log in to unmask] ______________________________ Reply Separator _________________________________ Subject: ASSY: Low Tin Level in Wave Solder Author: [log in to unmask] at ccmgw1 Date: 1/3/97 2:19 PM Good Day Everyone! We just got our solder analysis back (it's from a lab that everyone uses) for our wave solder pots, and we have one wave solder pot that's low in Tin... 61.4% to be exact. The recommendation is to add 4.3 lbs. of pure Tin for each 100 lbs. of solder to return it to the nominal 63%. My question is; just how in tarnation did we get one wave solder pot low on Tin? It don't make sense...we use the same bar solder in all our machines, we wave solder basically the same kinds of products in all of our machines. By that I mean we don't have one line waving only gold plated boards all the time, or only OSP coated PCB's all the time, etc.. so what gives? This is the very first time that I've ever had a solder analysis come back and tell me to put pure Tin into the pot...this is weird. I've had nickel get a little high before, but that's about it. We've got three machines and all of the analysis looks like this: Pot-1 Pot-2 Pot-3 Tin 62.4% 61.4% 62.7% Lead Balance Balance Balance Antimony <0.005% <0.005% <0.005% Copper 0.039% 0.048% 0.033% Gold 0.017% <0.003% <0.003% Silver <0.001% <0.001% 0.002% Aluminum <0.001% <0.001% <0.001% Arsenic <0.010% <0.010% <0.010% Bismuth 0.001% 0.001% <0.001% Cadmium <0.001% <0.001% <0.001% Indium <0.005% <0.005% <0.005% Iron <0.003% <0.003% <0.003% Nickel 0.006% 0.005% 0.004% Zinc <0.001% <0.001% <0.001% The analysis was conducted according to specifications in IPC-S-815B. As you can see, Pot-2 is the "slacker" tin-wise. The only noticable difference that I can see between the other two is that the copper content is just a tad higher...does that have anything to do with anything? Looking at the tin content on the other two pots, they're just barely above the limit which is 62.4%-63.6%...is my bar solder vendor starting to get tight with the Tin? Any light that anybody can shed on this would be 'preciated... __\/__ . / ^ _ \ . |\| (o)(o) |/| #------.OOOo----oo----oOOO.-----# # Steve Gregory # # SMT Process Engineer # # The SMT Centre Incorporated # # [log in to unmask] # #________________Oooo.__________# .oooO ( ) ( ) ) / \ ( (_/ \_) *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To unsubscribe from this list at any time, send a message to: * * [log in to unmask] with <subject: unsubscribe> and no text. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * *************************************************************************** *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To unsubscribe from this list at any time, send a message to: * * [log in to unmask] with <subject: unsubscribe> and no text. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************