Hi Bill Black To answer the questions you posed, and I forgot to save the message, we use CIBA Epibond 7275 Adhesive. a Stainless Steel, .008" thick Stencil, with .030" holes. The squegee is at 10 Lbs. The adhesive is heat cured. We use a Vitronics 20Zone, but just the front three zones, upper and lower, for the epoxy. Temps are 275C, 250C, 225C top/Bottom and belt at 12in/min. This epoxy sits for days on the stencil, with no problems. We are a single-shift shop, and the epoxy run can last all week. Then, the remaining goes into a jar, and is used next run. The Manu. Label says a shelf of 6 monthes, and its no joke. It lasts at least that long. Jack *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To unsubscribe from this list at any time, send a message to: * * [log in to unmask] with <subject: unsubscribe> and no text. * ***************************************************************************