Tom, I agree with your answer to small via's except for one important area. Small via's should NOT be allowed to be plated shut. As you know, the corners of the holes are high current areas and plate shut before the rest of the hole can close. This will result in the trapping of plating solutions (sulphuric acid and copper sulphate) in the middle of the hole that can leach out during the life of the board. To reduce the high current area, plating amperage may have to be reduced requiring longer plating cycles and increased board cost. IMO, tolerancing on via holes should be as follows: .018 +.003 minus .013 or .013 + .003 minus .008, etc., always leaving a hole open to a minimum of .005 for plating solutions to escape during HASL or any other surface finish. Then there should be another note on the drawing as follows: DO NOT PLATE THE HOLES CLOSED WITH COPPER. HOLES MAY BE FILLED WITH SOLDER AFTER REFLOW OR HASL. Norm Einarson Printed Circuit Technology *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To unsubscribe from this list at any time, send a message to: * * [log in to unmask] with <subject: unsubscribe> and no text. * ***************************************************************************