Martin, TCE of FR-4 would depend on whether it was difunctional, or multifunctional. Your laminate supplier should be able to give you specifics for your laminate. Here is something from my reference works. >From "Surface Mount Technology for PC Board Design", James K. Holloman, Jr: Properties of epoxy-glass: Glass transition temperature: 125C TCE and Y axis: 15 ppm/degreeC TCE Z axis: 48 ppm/degreeC Thermal conductance: 0.15 W/M*degreesC at 25 degrees C Dielectric contant at 1 MH: 4.8 >From "Printed Circuits Handbook", Clyde F. Coombs, Jr: Table 8.12 Coefficient of Thermal expansion - in inches/degree C x 1E-5 Lengthwise Crosswise FR-2 1.2 2.5 FR-3 1.3 2.5 CEM-1 1.1 1.7 CEM-3 1.0 1.5 FR-6 1.0 1.0 G-10 1.0 1.5 FR-4 1.0 1.5 G-11 1.0 1.5 FR-5 1.0 1.5 GI 1.0 1.2 This is based on the ASTM D696 test method. TCE is the change in length per degree change in temperature. The coefficient may vary in different temperature ranges, so the temperature range must be specified. Doug Pauls CSL [log in to unmask]