On 17 December, Ron wuz' wonderin': >> I would greatly appreciate any help I can get in reference to tombstoning >> of plastic film caps. My pad design for each terminal is .060" X .050". The >> .060" dimension is for width of the cap. Each terminal is centered on the >> .050", leaving .025" of the pad exposed on each side of the cap. We have to >> run the parts perpendicular to the direction of travel through the reflow >> because it is critical to the design. Please reply if anyone has experience >> with this. Thanks. Ron, Ain't that weird how them parts just wind-up standin' on their ends all by themselves? It's almost like there's some gremlins inside yer' oven with little gremlin tweezers standing yer' caps on their ends just trying ta' drive ya' crazy huh? Looking at yer' pad geometry's it don't seem like there's any big problem there...the gap between the pads don't seem excessive, and yer' sayin' that the part is centered-up on the pads prior to reflow...hmmmmm, there's a bunch of other things that might be causing this. Lemme' ask ya' a few more questions... I'm sure the other "Techie's" may have some of the same questions: 1. First thing, is the part okay? I mean as far as solderability... 2. What kinda' oven ya' got? Straight I/R, or Convection? 3. What's the profile set-points? 4. What else ya' got on the board? A lotta' IC's? or a bunch more passives? 5. How big is the board? How thick is it? Is there a lot of copper in the inner layers? (eg: heavy ground or power planes?) 6. How's the solder print? How thick are ya' printin' the paste? Are both pads equal and uniform in the paste deposit? For tombstoning to happen, something is causing the wetting forces acting on the component to become seriously unbalanced...it could be component solderabilty, or the timing is off when each pad becomes liquidous due to the profile or design variables in the PCB itself, or the solder deposition could be a factor too. I think the first place I would look though, is at yer' reflow profile. It's been my experience that most of the time that's what it's turned out to be. Do a plot and see that everything is in the window for an acceptable profile for the paste yer' using. Ya' know; "YER' BASIC PCB COOKIN' RECIPE" (For Medium-well done) Degrees C. 230 220 210 _-_<----Max peak 210-215 degrees C. 200 / -_ / \ _- \ _- \ 183-SN63 Solder melts _-<--Dwell at-->\ _- Liquidous \ 170 _- \ _------------- | 150 ,- | / <--Activators begin to react | 120 / | / | 100 / (Keep temperature ramp rates between 2-4 \ / degrees per second to avoid package cracking, \ 50 / solder balls, improper flux activity, or the | / dreaded "tombstones"!) \ 20 /_____________________________________________________\ | Phase-1 | Phase-2 | Phase-3 | Phase-4 | Phase-5 | | | | | | | Time:1-minute | 2-3 minutes | 30-seconds | 1-minute | to 1-minute Let us know what ya' find out.... __\/__ . / ^ _ \ . |\| (o)(o) |/| #------.OOOo----oo----oOOO.-----# # Steve Gregory # # SMT Process Engineer # # The SMT Centre Incorporated # # [log in to unmask] # #________________Oooo.__________# .oooO ( ) ( ) ) / \ ( (_/ \_) *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To unsubscribe from this list at any time, send a message to: * * [log in to unmask] with <subject: unsubscribe> and no text. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************