Dave, Very valid points! Technet, I would like to add one finding pertaining to solderability of electroless nickel - gold: Most have assumed the Phosphorus level is a major contributor to the solderability of this surface finish. Experiments completed in my past life have demonstrated that the nickel application process removes a portion of the copper, placing trace amounts of copper into the bath. Upon saturation, the copper is then re-depositied embedded in the nickel. The embedded copper oxidizes, making the surface unsolderable. Varying the levels of Phosphorus did not effect the solderability or yields during high volume experiments! Allen Hertz Racal-Datacom [log in to unmask] _______________________________________________________________________________ Subject: Re: solderability test for ENIG PCB finish Author: [log in to unmask] Date: 12/15/96 12:04 PM Good Morning TechNet! Your method of conducting a solderability test should not change just because you are not using a tin/lead finish! I suggest using one of the tests in ANSIJ-STD-003. With the emergence of the new alternative finishes (e.g. gold, silver, palladium) the specifications are still playing catch-up but the basic test methods are still applicable. You may need to change a dwell time because of dissolution rates (e.g. palladium) or may want to use a different flux because of your process (e.g. OSP type finishes) - work with your pwb vendor to have an acceptable test procedure both groups can use. I only have one reference in my pile of papers that discusses the relationship of solderability and E nickel but it's pretty good. Try: "Factors Influencing Solderability Of Electroless Ni-P Deposits", Jing Fang, Plating & Surface Finishing, pages 44-47, July 1992. Good Luck Dave Hillman Rockwell Collins [log in to unmask] ______________________________ Reply Separator _________________________________ Subject: solderability test for ENIG PCB finish Author: [log in to unmask] at ccmgw1 Date: 12/13/96 10:44 PM Dear Technetters, What is a quick, easy & effective way of assessing solderability/ wettability of a PCB with electroless nickel/immersion gold (ENIG) finish? How does phosphorus content in the Ni deposits affect solderability? Will a lower %P content in Ni be more prone to passivation/oxidation & thus affecting solderability?? *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To unsubscribe from this list at any time, send a message to: * * [log in to unmask] with <subject: unsubscribe> and no text. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * *************************************************************************** *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To unsubscribe from this list at any time, send a message to: * * [log in to unmask] with <subject: unsubscribe> and no text. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * *************************************************************************** *************************************************************************** * TechNet mail list is provided as a service by IPC using SmartList v3.05 * *************************************************************************** * To unsubscribe from this list at any time, send a message to: * * [log in to unmask] with <subject: unsubscribe> and no text. * *************************************************************************** * If you are having a problem with the IPC TechNet forum please contact * * Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask] * ***************************************************************************