Looks like "step plating". Residue from the resist developer were not removed by the pattern plate Pre-clean,. Hence copper does not plate right away and you end up with low spots. Eventually it starts plating so you don't end up with a total etchout. Small amounts around the edges of pads (seen only under magnification & a horizontal light source) is not that uncommon. ENIG of course makes any defect look worse. However this is pretty gross by any standards. Could also be some type of etch resist breakdown, but doubt it. Hope they are not ours! Robert E. Welch Senior Process Engineer Moog Components Group -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Wayne Thayer Sent: Wednesday, July 15, 2015 10:36 AM To: [log in to unmask] Subject: Re: [TN] MYSTRY DEFECT Some kind of weird pattern plating process defect? Light makes all defects of this type LOOK huge. IF the plating where the defects are is thinner than your specification for surface plating thickness, then it's rejectable. Measuring is easiest with a high resolution (>200X) optical microscope with a calibrated focus height readout. If used by a skilled operator, you can get a resolution of 3 microns or even a little better. If that's not good enough, you need to section and probably use SEM. Wayne -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory Sent: Wednesday, July 15, 2015 10:16 AM To: [log in to unmask] Subject: Re: [TN] MYSTRY DEFECT Hi Ong Seet Leng, I got your photos and have them posted now, the links are here: https://urldefense.proofpoint.com/v2/url?u=http-3A__stevezeva.homestead.com_Mystery-5FDefect-5F1.jpg&d=AwICaQ&c=ByDrzdYw8tO08sJlHDO_Vg&r=LW2JrkDqJ9rzfIEkoxZO_Q&m=jV6Qtbo-FApi-4a8NyqLiVdC-eocoheTAn7TCwH0-ZQ&s=9cXwBtf2TlJi1ADXmcnJ5CqFruSEe4Wm0xxOaCT-0Lk&e= https://urldefense.proofpoint.com/v2/url?u=http-3A__stevezeva.homestead.com_Mystery-5FDefect-5F2.jpg&d=AwICaQ&c=ByDrzdYw8tO08sJlHDO_Vg&r=LW2JrkDqJ9rzfIEkoxZO_Q&m=jV6Qtbo-FApi-4a8NyqLiVdC-eocoheTAn7TCwH0-ZQ&s=0c9kfnMi1Sy9OTIiPx0gJ2S1omgi-Ya2-hPd5umWKHc&e= Looks like there was some sort of problem with the etch resist, can't say exactly what that was though. I definitely would be kicking these back to the vendor! Steve On Tue, Jul 14, 2015 at 2:15 AM, Ong Seet Leng <[log in to unmask]> wrote: > Afternoon, > > I had checked a bare printed wiring board and attached a photograph on > one of the defect found. I would like to seek advice from you gurus' > out there on what to call this defect? For the life of me, I can't > find the definition of it. Appreciate if someone can guide me. Thanks > in advance. > > Regards, > Ong Seet Leng > > > > ______________________________________________________________________ > This email has been scanned by the Symantec Email Security.cloud service. > For more information please contact helpdesk at x2960 or > [log in to unmask] > ______________________________________________________________________ > -- This email and any attachments are only for use by the intended recipient(s) and may contain legally privileged, confidential, proprietary or otherwise private information. Any unauthorized use, reproduction, dissemination, distribution or other disclosure of the contents of this e-mail or its attachments is strictly prohibited. If you have received this email in error, please notify the sender immediately and delete the original. ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________