Hi Jim, I've attached a WORD file from back in 1999 that contains a little more information to support my assumption that the defects photos you sent to Steve are Foot-in-the-Mud defects. Regards, George George M. Wenger Failure Signature & Characterization Lab LLC 609 Cokesbury Road, High Bridge, NJ 08829 (908) 638-8771 Home (732) 309-8964 Mobile E-mail [log in to unmask] [log in to unmask] -----Original Message----- From: Wenger, George M. [Contractor] Sent: Tuesday, November 18, 2014 3:38 PM To: TechNet E-Mail Forum; Wenger, George M. [Contractor] Subject: RE: Solder defect Corner leads are also more likely to out of coplanarity than other leads, which also means a "Foot-in-the-Mud" defect is likely. Regards, George George M. Wenger Failure Signature & Characterization Lab LLC 609 Cokesbury Road, High Bridge, NJ 08829 (908) 638-8771 Home (732) 309-8964 Mobile E-mail [log in to unmask] [log in to unmask] -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M. [Contractor] Sent: Tuesday, November 18, 2014 3:28 PM To: [log in to unmask] Subject: Re: [TN] Solder defect Jim, This looks like a "Foot-in-the-Mud" defect. It could be caused by contamination but my best guess is it contamination isn't the cause. You need to determine (i.e., measure) the coplanarity of QFP leads and look at your assembly process to see if it can be tolerated. For example, if you are using a 5 mil thick stencil and the coplanarity of the QFN is above 3 or 4 mils you most likely have a "Foot-in-the-Mud" defect. Since solder paste is approximately 50% by volume metal and 50% flux vehicle and you look at it very simplistically when during reflow the flux vehicle becomes a fluid before the metal melts and you wind up with 2.5 mils of flux vehicle on 2.5 mils of metal and the lead that is 3 or 4 mils above the others will be sitting is flux and when the solder melts it doesn't jump up through the flux to touch and wet the lead. So what you are left with is an imprint of the foot of the lead in the solder that wet to the pad but not the lead. Regards, George George M. Wenger Failure Signature & Characterization Lab LLC 609 Cokesbury Road, High Bridge, NJ 08829 (908) 638-8771 Home (732) 309-8964 Mobile E-mail [log in to unmask] [log in to unmask] -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Jim West Sent: Tuesday, November 18, 2014 3:13 PM To: [log in to unmask] Subject: [TN] Solder defect Hi all, Please see attached links. (Thanks Steve) http://stevezeva.homestead.com/IMG00002.jpg http://stevezeva.homestead.com/IMG00004.jpg http://stevezeva.homestead.com/IMG00008.jpg We have recently come across two failures that were the result of one (1) pin not soldered on a 144 pin QFP. Looking at the pictures, you'll see no wetting and the pin embedded in the solder. We could say it's contamination, but we had no issues with any other pins on the QFP. One more thing to add to the troubleshooting, the failure is the same pin (36) on the QFP. Do I have a warping issue? The pin doesn't appear to be bent, but I have not ruled that out until I have better means of verifying. If it's contamination, why only one pin? I would think that I would get at lease the heel or toe, or even the sides to solder, but in this case no wetting. You can see the pin has made contact with the solder due to the indentation. How does this not solder if it has made contact with the solder paste? I'm at a loss and we will probably end up sending this to a lab, but I'm not sure if we will gain anything from a lab?? We are using leaded solder for this application. Photo IMG00002 and 00004 are from the same failure Photo IMG00008 is the 2nd failure. Your thoughts? Thanks, Jim ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________