robert. Deactivation temperature do exist, if you are part of team developed formulation. The conversion of active species after the oxide removal task of flux can be neutralized by additional chemical species (usually a compound complex to take off the acid in the flux at some temperature and time). No body is going to tell you how it works (most likely trade secrete if not patented). The clue of how to use it properly is usually in the application notes of the flux (if you get from the maker, not the distributor). Or some vendor's application engineer will develop your process and tell you what would be the most likely best solution for your application (at cost of course). you still need validated by yourself, via testing. That is why you do not want to change flux often (a few cents cheaper is not a good reason to change flux). If you got chance to work with a chemist at vendor site, provide you have large enough order to justify, you might know a bit and pieces.... Currently, most of MFG are on contract and far far away from the selection of material, all the details are lost in translation.. tough luck for you if you need to optimize "no-clean". my 2 cents. jk On Sep 8, 2014, at 12:19 PM, Robert Kondner wrote: > Dave, > > Yes, there are plenty of adequate tool within the industry to > determine if a flux residue has an unacceptable ionic content. > > But it seems like some folks don't give a darn if either: > > 1 The flux is called "No-Clean" even by a competent manufacturer > engineer. Or if a No-Clean flux residue has been measured as > acceptable the adequate tools. > > 2 The flux has never been heated past some imaginary "Deactivation > Temperature" that no competent manufacture seems to spec in the > first place. Yet we are told to believe the competent manufacturers > application information. > > We live or die by making measurements with accurate tools. To > ignore these on a personal whim is just plain nonsense. If we > believe in "Deactivation Temperature Processing" as a way of > meeting some ionic contamination spec we just might end up wishing > there was deactivation temps for pink slips. (I hear bleach works.) > > And if we don't believe in "Deactivation Temperature Processing" > why are we even having this discussion? > > So I am over and out on this. > > Bob K. > > -----Original Message----- > From: TechNet [mailto:[log in to unmask]] On Behalf Of David Hillman > Sent: Monday, September 08, 2014 11:34 AM > To: [log in to unmask] > Subject: Re: [TN] tinning wires - flux entrapment and long term > reliability > > Hi Bob - there are adequate tools within the industry to determine > if a flux residue has an unacceptable ionic content - Ion > Chromatography, SIR, specific dielectric functionality testing, > etc. so determining if your flux and process are compatible is > simple -lots of work but simple. Many, many products utilize a "no > clean" process using "low residue" flux materials very successfully > so it is not hogwash but just good materials & process engineering. > Of course, if someone does implement a "no clean" process without > doing their due diligence homework and testing, yes, they are not > going to be happy with the result. > > Dave > > On Mon, Sep 8, 2014 at 10:15 AM, Robert Kondner > <[log in to unmask]> > wrote: > >> Dave, >> >> Maybe it is "Fundamentally" a bit of hog wash. :-) >> >> The comments that started to thread was your description of why rosin >> based flux was good in the use of wire prep. I your description >> sounds >> reasonable to me. >> >> Richard also seemed to find you information interesting. >> >> But that thread starting point mentioned the use of RMA but never to >> use a "No Clean" flux. That sounds silly to me. If a manufacturer >> put >> that same RMA flux in a bottle and called it "No Clean" I guess it >> would then never be used? >> >> And then I was told to follow the manufacturer's advice! (Maybe that >> means as long as the manufacturers advice is not "No Clean".) >> (Hmmm is >> Not "No-Clean" = Clean Always?) >> >> So I am back to the point of: >> >> 1. Read the Label >> >> 2. Follow the recommended processes. (And that included cleaning, if >> any.) >> >> 3. If you are not cleaning off flux (or you cannot due to >> entrapment) >> double check everything. Use RMA or No Clean. >> >> But to have people poo-poo a No Clean as it has not been >> "Deactivated" >> through proper temperature is not verifiable. And until there is >> competent advice to be found the idea falls into the hogwash >> category. >> >> Just Say No to Hogwash. >> >> Thanks, >> Bob >> >> -----Original Message----- >> From: TechNet [mailto:[log in to unmask]] On Behalf Of David Hillman >> Sent: Monday, September 08, 2014 10:43 AM >> To: [log in to unmask] >> Subject: Re: [TN] tinning wires - flux entrapment and long term >> reliability >> >> Hi Bob - as Richard detailed, you need to get down to the flux >> supplier application engineers for that detail of information. And >> nope, I don't have a clue on why something so fundamental isn't a >> standard data point on the tech data sheet. >> >> Dave >> >> On Mon, Sep 8, 2014 at 9:28 AM, Robert Kondner >> <[log in to unmask]> >> wrote: >> >>> Dave, >>> >>> I did look into this issue, several times. I still sense a bit of >>> "Hog Wash" on this subject. I am trying to separate the hogs here. >>> >>> Go take a look at the Kester 951 data sheet. No "Deactivation >>> Temperature" spec there. >>> >>> Go take a look at Kester 2331-ZX, now this stuff you need to >>> clean. >>> Again no "Deactivation Temperature" specified. >>> >>> So I suggest you get ahold of some flux supplier application folks >>> and ask them for "Minimum Processing Temperature for Flux >>> Deactivation". I don't think you will find such a specification. >>> >>> Thanks, >>> Bob K. >>> >>> >>> >>> -----Original Message----- >>> From: TechNet [mailto:[log in to unmask]] On Behalf Of David Hillman >>> Sent: Monday, September 08, 2014 10:10 AM >>> To: [log in to unmask] >>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>> reliability >>> >>> Hi Bob - as Richard detailed, if you get ahold of the flux supplier >>> application folks, they have the necessary data for setting up an >>> adequate profile and temperature range, application depenedent. The >> whole "no clean" >>> topic drives me batty - the proper term is "low residue" as I don't >>> have my flux suppliers dictating when I should or should not clean. >>> A case of marketing edging out engineering on the correct use of >>> technical >> terms. >>> >>> Hey Doug - didn't you and Bill Kenyon have a nice synopsis on the >>> "no clean vs low residue" topic? >>> >>> Dave >>> >>> On Mon, Sep 8, 2014 at 8:57 AM, Robert Kondner >>> <[log in to unmask]> >>> wrote: >>> >>>> Dave, >>>> >>>> Ok, so if a manufacturer says a flux is categorically "No Clean" >>>> we should believe it, right? :-) >>>> >>>> Offhand I never recall seeing a Minimum Temperature specification >>>> for the use of any flux. I recall finding usage temperature >>>> ranges, and you find info on how long the flux is active, find >>>> statements about must be cleaned or no clean, but have you ever >>>> seen a flux with a minimum processing window to be qualified as >>>> a "No Clean"? >>>> >>>> From experience I know that heating profiles of PCB assemblies in >>>> reflow ovens are selected such that all the flux does not >>>> completely >>> "Burn Off". >>>> In fact profiles where the flux remains active is what helps make >>>> nice shiny solder joints, everyone loves those. >>>> >>>> I have not seen one shred of evidence in flux usage information >>>> that suggest leaving flux residue is safe IF it has been heated to >>>> some temperature for some specific length of time. All I see are >>>> fluxes listed as "Must Clean" or "No Clean". >>>> >>>> Do you know of any flux called "You Might Need to Clean"? >>>> >>>> Bob K. >>>> >>>> >>>> -----Original Message----- >>>> From: TechNet [mailto:[log in to unmask]] On Behalf Of David Hillman >>>> Sent: Monday, September 08, 2014 9:23 AM >>>> To: [log in to unmask] >>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>> reliability >>>> >>>> Hi Bob - all fluxes have a temperature range, or at least a >>>> minimum temperature value, that they should be heated to to >>>> accomplish two >> tasks: >>>> (1) attack/remove the oxides that inhibit the formation of a good >>>> solder wetting; (2) decompose the activators such that they are >>>> benign in the flux residue. The flux suppliers know their >>>> formulations and can provide temperature recommendations to ensure >>>> we can create adequate reflow profiles in our processes. >>>> >>>> Dave >>>> >>>> On Mon, Sep 8, 2014 at 7:58 AM, Robert Kondner >>>> <[log in to unmask]> >>>> wrote: >>>> >>>>> Richard, >>>>> >>>>> So, I ask: >>>>> >>>>> Does a rosin based "No Clean" flux need to be completely >>>>> heated to high temperature to "De-Activate" the flux? >>>>> >>>>> If what Dave say is correct the answer is no. I think? >>>>> >>>>> Bob K >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, >>>>> Richard >> D. >>>>> Sent: Monday, September 08, 2014 8:29 AM >>>>> To: [log in to unmask] >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> Dave, I never knew that about RMA fluxes. This is valuable >>>>> information, and I thank you for it. >>>>> dean >>>>> >>>>> From: David Hillman [mailto:[log in to unmask]] >>>>> Sent: Friday, September 05, 2014 4:03 PM >>>>> To: TechNet E-Mail Forum; Stadem, Richard D. >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> Hi Richard - I can provide some additional information. The >>>>> value of rosin based fluxes is that when using the proper >>>>> soldering temperatures and dwell times, the resulting flux >>>>> residues are not mobile, ionic species that can participate in >>>>> corrosion reactions (note that there is always an exception to >>>>> the rule). The rosin portion of rosin based fluxes can "bind up" >>>>> any mobile, ionic species if they are not completely consumed in >>>>> the soldering reaction. That is why rosin based fluxes are very >>>>> robust in soldering processes. As George and others detailed, >>>>> "no clean' is a horrible material descriptor as it is a process >>>>> categorization rather than a material categorization. The better >>>>> term is "low residue" and as others detailed, not all low >>>>> residue materials are created equal. Many low residue fluxes are >>>>> rosin based materials so they have applicability for wiring >>>>> tinning but an engineer has to do their homework to make sure >>>>> there is process compatiblilty. >>>>> And yes, when folks attempt to use water soluble fluxes in the >>>>> same manner as rosin fluxes, bad things happen. The wire >>>>> tinning process you learned has its credibility in the rosin >>>>> chemistry (the IPA relavence isn't as critical >>>> or necessary as Brian can/has detailed) and is supported by the >>>> products you detailed. >>>>> >>>>> I believe Doug and Bill Kenyon put together a "letter" on this >>>>> topic and I'll see if Doug can find that for posting thru Steve. >>>>> >>>>> Dave Hillman >>>>> Rockwell Collins >>>>> [log in to unmask]<mailto:david.hillman@rockwellc >>>>> ol >>>>> li >>>>> ns >>>>> .com >>>>>> >>>>> >>>>> On Fri, Sep 5, 2014 at 3:00 PM, Stadem, Richard D. < >>>>> [log in to unmask]<mailto:[log in to unmask]>> >>>>> wrote: >>>>> I started out in life as a small child with a very large pair of >>>>> safety glasses and a leather apron, tinning wires in my father's >>>> business. >>>>> I later re-learned how to do this from two much older engineers, >>>>> who had retired from RCA and Honeywell, and they had been using >>>>> this method since they were little boys in their father's shop. >>>>> I have also taught this method to my three sons, as there still >>>>> seems to be no end of wire tinning requirements even today. >>>>> >>>>> 1. When stripping the wires, leave the tag end of the insulation >>>>> hanging on the end of the wire. This helps prevent the strands >>>>> from fraying during handling. >>>>> 2. When ready, pull off the tag end of the insulation. Dip the >>>>> stripped end of the wire first in IPA up to the end of the >> insulation. >>>>> 2. Then dip the wire in the RMA flux up to about halfway to the >>>>> insulation. Use only RMA flux whenever tinning wires, never OA >>>>> or water soluble flux, and never no-clean flux. >>>>> 3. Then dip the fluxed end into the solder right up to within . >>>>> 010" >>>>> from the insulation and hold for 1 or 2 seconds. This allows the >>>>> solder to wick just under the insulation. >>>>> 4. Pull the wire out of the solder and "swirl" in clean IPA, and >>>>> then lay the wires down flat on a piece of absorbent paper towel. >>>>> 5. If an ultrasonic cleaner can be used, ie, the wires are not >>>>> soldered to any CCA or any electronic components, then instead >>>>> of laying them on the paper towel, drop them into the US cleaner >>>>> with a solution of 90% DI water and 10% IPA. Do not exceed the >>>>> 10% IPA percentage or you will have a new company swimming pool, >>>>> but also you will be minus a few operators and you will gain >>>>> many new friends at OSHA and Davidovich, Davidovich, and >>>>> Rabinovitch, Atty's >> at Law. >>>>> 6. Once all of the wires have been cleaned for a minimum of 10 >>>>> minutes in the US bath, take them out and dry them on a clean >>>>> paper >>> towel. >>>>> >>>>> This is a time-tested method, dating back to the late 1950s. >>>>> >>>>> My understanding (and it may be flawed) is that RMA is used >>>>> because even if small amounts are not dissolved in the IPA, >>>>> whatever residues that do remain are relatively harmless, >>>>> because they are weakened by the IPA already in the wire >>>>> strands, and after tinning, most if not all is removed during >>>>> the "swirling" in IPA. When the wires are laid down on the paper >>>>> towel, the IPA and the flux solids are drawn out, and any >>>>> remaining residues left behind are relatively >>> harmless. >>>>> >>>>> I do know that this method of tinning wires was used in the old >>>>> Apollo program. >>>>> It was also used on the Neartip Mark 5 Torpedo Guidance and >>>>> Control systems. >>>>> It was also used on the older Mark 2 Torpedoes. >>>>> It was also used on the Advanced Lightweight Torpedo. >>>>> It was used on the Apache, C5B, Augusta, F-15, F-16, FA-18 >>>>> avionics systems, including the flight control computers, the >>>>> ring laser gyros, the altimeters, the wind speed indicators, the >>>>> flapper controls, the CMRA and HMRA Cruise Missiles, The >>>>> CH46/CH47 avionics sets, the Space Shuttle wiring, and about >>>>> 400-500 commercial jet plane >>> wiring sets. >>>>> >>>>> I have yet to hear of any wires broken off from corrosion under >>>>> the insulation. >>>>> >>>>> I have heard of many wires corroding away because either water >>>>> soluble flux or no-clean fluxes were used. Water soluble fluxes >>>>> do not wash out or dilute when dipped in alcohol or water (at >>>>> least not very well). Ditto with no-clean fluxes. >>>>> >>>>> >>>>> My only concern is that there are RMA fluxes, and there are RMA >>>>> fluxes, and some may be more aggressive than others. >>>>> >>>>> >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Nutting, Phil >>>>> Sent: Friday, September 05, 2014 11:56 AM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> Dusting off an old thread here (yes Brian, I listened to your >>>>> request for not changing threads). I've been thinking about the >>>>> "best" method of wire tinning for some time now and this thread >>>>> makes me think the we should dump our no-clean cored wire solder >>>>> in favor of something that >>>> is more innocuous. >>>>> >>>>> I have an old roll of Kester 63/37 "44" core saved from years >>>>> ago before the switch to lead-free. Is this acceptable for long >>>>> term soldered wire reliability. If not, what are the >>>>> recommendations? >>>>> I guess knowing RA or RMA along with manufacturer and "model" >>>>> would be useful. Hopefully it is available in 63/37 and >>>>> lead-free >> alloys. >>>>> >>>>> Thanks in advance for sharing your knowledge and experience, >>>>> >>>>> Phil Nutting >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Carl VanWormer >>>>> Sent: Tuesday, June 10, 2014 11:55 AM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> There sure are a lot of scare stories about flux and reliability. >>>>> I'm now wondering if a solution based on crimping some sort of >>>>> ferrule or machined pin onto the ends of the wires and then >>>>> soldering those metal parts into the PCB holes might be a more >>>>> reliable approach. Have any of >>>> "you guys" >>>>> seen that type of solution to this problem? >>>>> >>>>> Thanks, >>>>> Carl >>>>> >>>>> >>>>> Carl B. Van Wormer, P.E., AE7GD >>>>> Senior Hardware Engineer >>>>> Cipher Engineering LLC >>>>> 21195 NW Evergreen Pkwy Ste 209 >>>>> Hillsboro, OR 97124-7167 >>>>> 503-617-7447x303<tel:503-617-7447x303> >>>>> >>>>> [log in to unmask]<mailto:[log in to unmask]> >>>>> http://cipherengineering.com >>>>> >>>>> >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Karen Tellefsen >>>>> Sent: Tuesday, June 10, 2014 6:00 AM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> I would use Kester 186-18 instead for tinning. Alpha 615-15 is >>>>> another good choice. >>>>> >>>>> Karen Tellefsen - Electrical Testing Alpha / 109 Corporate >>>>> Blvd./ S. >>>>> Plainfield, NJ 07080 [log in to unmask] >>>>> <mailto:[log in to unmask]> 908-791-3069<tel:908-791-3069> >>>>> >>>>> >>>>> >>>>> >>>>> From: Steve Gregory >>>>> <[log in to unmask]<mailto:[log in to unmask] >>>> >>>>> To: <[log in to unmask]<mailto:[log in to unmask]>>, >>>>> Date: 06/09/2014 05:43 PM >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long >> term >>>>> reliability >>>>> Sent by: TechNet <[log in to unmask]<mailto:[log in to unmask]>> >>>>> >>>>> >>>>> >>>>> Hi Richard, >>>>> >>>>> Good information! But can I ask a question about a particular >>>>> no-clean flux? It's about Kester 951. In their datasheet they >>>>> say that it contains a "corrosion inhibitor" such that no >>>>> corrosion products are formed when bare copper surfaces are >>>>> exposed to humid environments. Do you have any idea what that >>>>> might be? >>>>> >>>>> We use it as a touch-up flux for our no-clean soldering and do >>>>> use it to tin wires. I know that some of that flux gets >>>>> somewhere where it doesn't get cleaned, and probably didn't get >>>>> exposed to a lot of heat when you're doing point-to-point >>>>> touch-up and soldering with a single >>>> iron. >>>>> >>>>> We haven't had an issue with this flux, at least any that I >>>>> know of. >>>>> But it doesn't mean that there isn't one. The operators >>>>> sometimes complain when they use it because it evaporates so >>>>> fast though. >>>>> >>>>> Just curious what the "corrosion inhibiter" might be. The SDS >>>>> says the flux contains ethanol (50-65%), isopropanol (20-25%), >>>>> n-butyl acetate (5-10%), methanol (2.5-5%), and adipic acid >>>>> (1-2.5%). >>>>> Everything listed is pretty much a solvent except for the adipic >> acid. >>>>> >>>>> Steve >>>>> >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Stadem, Richard D. >>>>> Sent: Monday, June 9, 2014 2:23 PM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> I agree with George, and also with many others who feel that >>>>> cleaning with IPA is not a very good approach. >>>>> I should have mentioned also that through the years that I have >>>>> seen wires tinned with RMA flux, then soaked in IPA, then that >>>>> was followed by a DI wash. >>>>> >>>>> The old-time engineers back in the 60s and 70s showed me by >>>>> using >>>>> 3 stages of wires cut open to show what the strands looked like >>>>> under the insulation. Different oldtimers showed me this trick >>>>> more than once, and I have never forgotten it. >>>>> >>>>> First, the operators were trained to insert the wires into the >>>>> RMA flux only halfway up the stripped portion (generally 1/8th >>>>> inch to >> 1/4" >>>>> striplength). >>>>> Next, the operator was trained to insert the wire only up to >>>>> just below the end of the insulation. Some of the RMA flux would >>>>> always ride up to the insulation, and the solder would actually >>>>> flow just under the insulation, seldom more than .050" past the >>>>> end of the insulation. In other words, if you stop the stranded >>>>> wire just short of the insulation, the solder continues to wick >>>>> up to a point just under >>>> the end of the insulation. >>>>> Then, when the wires were not cleaned with IPA at all, the >>>>> cutaway view would always show a small amount of flux just under >>>>> the end of the insulation. >>>>> When cleaned in the IPA only, but not followed with a water >>>>> wash, when you cut the insulation away you "sometimes" saw a >>>>> very small amount of >>>> flux. >>>>> But when you did all three, any flux residue under the >>>>> insulation (if >>>>> present) could not be seen. It does not mean it wasn't there; it >>>>> just was not visible even at 20X. >>>>> >>>>> And in all cases, the oldtimers were never concerned with RMA >>>>> flux residues being left behind under the insulation; they felt >>>>> it was not a concern even to leave the RMA flux behind, with no >>>>> cleaning. >>>>> >>>>> But NOT water soluble (OA) and NOT no-clean fluxes. The no-clean >>>>> activators are sometimes even more aggressive than RMA. That is >>>>> still >>>> true. >>>>> So I stand by the statement that when tinning wires, only RMA >>>>> flux should be used, some type of solvent should be used to at >>>>> least suspend the RMA solids, and some type of final rinse or >>>>> wash process should be used. If all of those are done, I do not >>>>> think there is ever a concern for the wires rotting away under >>>>> the >> insulation. >>>>> >>>>> And one more item: If you are just cleaning tinned wires (no >>>>> connector bodies, sleeving, circuit boards or components,etc.) I >>>>> have found that following the solvent clean with an ultrasonic >>>>> cleaning process where the entire wire or wire assembly is >>>>> immersed in hot DI water with a 6% saponifier will get all of >>>>> the flux out from under the end of the insulation. >>>>> >>>>> I am talking about the end of the insulation, not 1/2" up the >>>>> insulation or anything like that. >>>>> >>>>> >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Wenger, George M. >>>>> [Contractor] >>>>> Sent: Monday, June 09, 2014 1:21 PM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> As someone who sent 33 years working in the "Bell System" were >>>>> solder assembly quality/reliability was the primary concern, >>>>> I'll throw my two cents into this discussion. I've never like >>>>> the name >>> "No-Clean". >>>>> Any flux used for soldering that doesn't go through a cleaning >>>>> process would be a "No-Clean" if the meaning is it wasn't >>>>> cleaned off. The old BellCore (now >>>>> Telcordia) GR-78 gives criteria for determining if a soldering >>>>> flux residue needs to be cleaned off for reliability reasons. >>>>> If you make a solder joint with a flux and don't clean it off >>>>> and it passes the BellCore reliability testing then we would >>>>> consider that flux a reliable "Leave-Behind" flux meaning if the >>>>> flux residue wasn't cleaned off there were no reliability risks. >>>>> In general most of the old fluxes classified as R & RMA passed >>>>> the >> "leave-Behind" >>>>> requirement. In fact, our experience was that especially for >>>>> RMA fluxes the reliability was much better if you did leave them >>>>> behind rather than tried to clean them. If you take an RMA flux >>>>> and try cleaning it with alcohol (which isn't a very good >>>>> solvent) what you wind up doing is dissolving and removing most >>>>> of the rosin in the flux residue, which is what was >>>>> encapsulating the ionic activators, which in turn allowed any >>>>> ionic activators to be mobile and the first time the humidity >>>>> increased you had the worse case for corrosion (moisture, >>>> activators, and electrical potential). >>>>> >>>>> I can see that with a low-solids type "No-Clean" flux that the >>>>> flux would wick up the braided wires and yes when a soldering >>>>> iron was placed on where you wanted to make the solder joint the >>>>> flux activators would be heated and reduce oxides and allow a >>>>> good solder joint to form but the flux that wicked up the wires >>>>> may not have gotten to a high enough temperature to de-activate >>>>> the activators and then the humidity goes up in use you could >>>>> have a problem. If I were pre-tinning braided wires I would >>>>> only us an RMA flux qualified >>>> according to BellCore GR-78 to be a "Leave-Behind". >>>>> >>>>> Regards, >>>>> George >>>>> George M. Wenger >>>>> Failure Signature & Characterization Lab LLC >>>>> 609 Cokesbury Road, High Bridge, NJ 08829 >>>>> (908) 638-8771<tel:%28908%29%20638-8771> Home (732) >>>>> 309-8964<tel:%28732%29%20309-8964> >>>>> Mobile E-mail >>>>> [log in to unmask]<mailto:[log in to unmask]> >>>>> [log in to unmask]<mailto:[log in to unmask]> >>>>> >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Carl VanWormer >>>>> Sent: Monday, June 09, 2014 12:59 PM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> I've heard stories of no-clean and hand soldering causing >>>>> problems. >>>>> In an IR-reflow oven, all of the no-clean flux achieves the >>>>> passivation temperature, becoming inert. With hand soldering, >>>>> the flux melts, runs away from the heat source, and penetrates >>>>> any tiny >>>> crevice it can find. >>>>> There is an area at the perimeter of the heated area that is hot >>>>> enough to cause the flux to flow, but not hot enough to cause it >>>>> to >>>> become active. >>>>> If this is true, than this is the problem I'm worried about. >>>>> Comments, please? >>>>> >>>>> Thanks, >>>>> Carl >>>>> >>>>> >>>>> >>>>> Carl B. Van Wormer, P.E., AE7GD >>>>> Senior Hardware Engineer >>>>> Cipher Engineering LLC >>>>> 21195 NW Evergreen Pkwy Ste 209 >>>>> Hillsboro, OR 97124-7167 >>>>> 503-617-7447x303<tel:503-617-7447x303> >>>>> >>>>> [log in to unmask]<mailto:[log in to unmask]> >>>>> http://cipherengineering.com >>>>> >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Steve Gregory >>>>> Sent: Monday, June 09, 2014 9:49 AM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> It's been some years back, but we were building a cabinet along >>>>> with all the boards and cables. The cables had silver plated >>>>> braided shielding over them and we would have to solder the >>>>> shield wires to either a lug or contact. We were using >>>>> manufacture XXX >> no-clean flux. >>>>> It had been a rainy spring that year, and rained about every >>>>> other day for at least a month, so you know the humidity was high. >>>>> >>>>> One of the supervisors came to me after that month and said; >>>>> "Steve, we got a problem, all the cables in the cabinets are >>>>> turning >> green..." >>>>> so I went and looked at them. Sure enough the shield wires were >>>>> turning green, and it was down close to the end sections of the >>>>> cables where they had been >>>>> soldered: >>>>> >>>>> http://stevezeva.homestead.com/files/Green_Junk_1.jpg >>>>> >>>>> http://stevezeva.homestead.com/files/Green_Junk_2.jpg >>>>> >>>>> http://stevezeva.homestead.com/files/Green_Junk_3.jpg >>>>> >>>>> http://stevezeva.homestead.com/files/Green_Junk_Close.jpg >>>>> >>>>> I had a hard time figuring out how this was happening, because >>>>> right at the ends where the soldered connection it was fine. The >>>>> connections were soldered and cleaned with alcohol. Best I could >>>>> figure was that the operators had flux on their fingers when >>>>> they handled the cables and got the flux up on the cable where >>>>> it wasn't reacted with heat, and wasn't cleaned, and with the >>>>> high humidity that we had that month turned the shield wire green. >>>>> >>>>> We switched the no-clean flux to manufacture XXX and the problem >>>>> went >>>> away. >>>>> >>>>> Steve >>>>> >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Nutting, Phil >>>>> Sent: Monday, June 9, 2014 8:25 AM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> So for many years I have followed the discussion about flux >>>>> cleaning and alcohol always get mentioned as a great way of >>>>> dissolving the flux and depositing it on a much wider area. >>>>> There has to be a better way to "clean" the wire entrapped flux >>>>> if it really must be cleaned. I agree that OA flux is not a >>>>> good solution. My current choice is to use >>>> "no-clean" >>>>> flux cored solder when tinning wires and then leave it alone. >>>>> Soldering the wire into the board can then be done with "no-clean" >>>>> or other flux cored solder. Where we do not make anything that >>>>> is designed as mission critical this process seems to work for us. >>>>> >>>>> Phil Nutting >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Stadem, Richard D. >>>>> Sent: Monday, June 09, 2014 9:30 AM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: Re: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> You do not tell us what flux you are using. >>>>> But as a general rule, one must never tin insulated wires using >>>>> OA >>> flux. >>>>> Only RMA or no-clean should be used, and that followed by >>>>> dipping the tinned ends in alcohol. >>>>> >>>>> >>>>> -----Original Message----- >>>>> From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] >>>>> On Behalf Of Carl VanWormer >>>>> Sent: Friday, June 06, 2014 8:20 AM >>>>> To: [log in to unmask]<mailto:[log in to unmask]> >>>>> Subject: [TN] tinning wires - flux entrapment and long term >>>>> reliability >>>>> >>>>> My understanding: >>>>> While tinning wires with conventional soldering methods, the >>>>> wire is heated and the flux-cored solder is applied to the wire. >>>>> As the flux is melted, it wicks up between the wires and the >>>>> solder flows in, wetting the wires. The liquefied flux flows up >>>>> the wires farther than the solder, and some of the un-passivated >>>>> flux is trapped inside the insulation, around the Copper strands >>>>> where the >>> solder stopped flowing. >>>>> >>>>> My experience: >>>>> One of our control modules had failed in an automotive "road >>>>> splash" >>>>> environment. Our connector terminals had been soldered to the >>>>> wires that came out of the "waterproof" strain-relief assembly. >>>>> Troubleshooting let me to cable harness with an open circuit >>>>> between a wired connector pin and the other end of the wire. >>>>> The wire and pin looked good, but a gentle tug on the pin popped >>>>> the 5mm length of soldered wire out of the wire's insulation, >>>>> revealing a discoloration at the end of the solder-flow where >>>>> the Copper wire had been >>>> "disappeared". >>>>> A few mm inside the wire insulation, there was another >>>>> discolored blob at the end of the wire's total length of good >>>>> Copper wire. >>>>> Our conclusions of "not quite waterproof" and "chemistry >>>>> experiment" led me to be concerned about the problem. >>>>> >>>>> Current worry: >>>>> We have a product with a "requirement" that some 16-gauge >>>>> stranded Copper wires be soldered to our PC board. The plan is >>>>> to have the cable assembly arrive with pre-tinned wires, and >>>>> then the wires will be soldered to the board with "no-clean" >>>>> flux. The product is not expected to be in the water, but may >>>>> be "near" a wet environment, maybe mounted in a pouch on some >>>>> motorcycle gear. >>>>> I'm worried about the tinning process forcing un-passivated flux >>>>> up, inside the >>>> insulation, to wait for a "humid" >>>>> condition to start another "chemistry experiment." >>>>> >>>>> Questions: >>>>> >>>>> 1. Assuming we must solder wires to my PC board, is there >>>>> any >>>>> guidance on how to keep "chemistry experiments" from happening >>>>> on my product? >>>>> >>>>> 2. Are there any other "very small" connection methods >>>>> for 15 >> Amp >>>>> wires that I should consider that I might be able to fit on my >>>>> tiny PC board that would eliminate my worry? >>>>> >>>>> 3. Am I just being overly paranoid? >>>>> >>>>> Thanks, >>>>> Carl >>>>> >>>>> >>>>> >>>>> >>>>> >>>>> Carl B. Van Wormer, P.E., AE7GD >>>>> Senior Hardware Engineer >>>>> Cipher Engineering LLC >>>>> 21195 NW Evergreen Pkwy Ste 209 >>>>> Hillsboro, OR 97124-7167 >>>>> 503-617-7447x303 >>>>> [log in to unmask]<mailto:[log in to unmask] >>>>> <mailto: >>>>> [log in to unmask]<mailto:[log in to unmask]>> >>>>> http://cipherengineering.com<http://cipherengineering.com/> >>>>> >>>>> This message may contain confidential and/or proprietary >>>>> information, and is intended for the person/entity to whom it >>>>> was originally addressed. Any use by others is strictly >>>>> prohibited. >>>>> If I sent this to you by mistake, please be nice and delete it, >>>>> and then tell me of my mistake so I can send it to the right >>>>> person. >>>>> >>>>> >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> >>>>> >>>>> >>>>> ***** Please note that my E-Mail address has changed ***** >>>>> >>>>> ________________________________________________________________ >>>>> __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud >>> service. >>>>> For more information please visit http://www.symanteccloud.com >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] <mailto:[log in to unmask]> >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>>> ________________________________________________________________ >>>>> __ __ __ This email has been scanned by the Symantec Email >>>>> Security.cloud service. >>>>> For more information please contact helpdesk at x2960 or >>>>> [log in to unmask] >>>>> ________________________________________________________________ >>>>> __ >>>>> __ >>>>> __ >>>>> >>>> >>>> >>>> __________________________________________________________________ >>>> __ __ This email has been scanned by the Symantec Email >>>> Security.cloud service. >>>> For more information please contact helpdesk at x2960 or >>>> [log in to unmask] >>>> __________________________________________________________________ >>>> __ >>>> __ >>>> >>>> >>> >>> >>> ____________________________________________________________________ >>> __ This email has been scanned by the Symantec Email Security.cloud >>> service. >>> For more information please contact helpdesk at x2960 or >>> [log in to unmask] >>> ____________________________________________________________________ >>> __ >>> >>> >> >> >> _____________________________________________________________________ >> _ >> This email has been scanned by the Symantec Email Security.cloud >> service. >> For more information please contact helpdesk at x2960 or >> [log in to unmask] >> _____________________________________________________________________ >> _ >> >> > > > ______________________________________________________________________ > This email has been scanned by the Symantec Email Security.cloud > service. > For more information please contact helpdesk at x2960 or > [log in to unmask] > ______________________________________________________________________ > > ______________________________________________________________________ > This email has been scanned by the Symantec Email Security.cloud > service. > For more information please contact helpdesk at x2960 or > [log in to unmask] > ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________