Phil, By any chance is your in-house using an air knife or similar to remove excess wash water and is another group (CM) allowing to dry? I did some playing with remaining residue and if folks wash with tap water, and blow off excess water, the surface contamination will appear very low. But a single tiny drop of water in the wrong place could be a problem. Worse Yet even rinses with DI will not clean under a QFN. And tiny drops of DI get to tape water equivalent with even tiny tiny amounts of dissolved material. If you think about flux getting cooked into nooks and crannies what good is a DI wash/ You relly might need an additive that reduces surface tensions of the wash water. But now that stuff is in there. Can't Win. Also, you mention opto devices and between the various grades (transfer efficiency), vendors, user designs and ageing many of an opto isolation circuits "Go Bad" because the designer did not account for all the operating parameters. I know, been there and done that. They are not easy to use devices. Bob K. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Nutting, Phil Sent: Thursday, July 31, 2014 10:38 AM To: [log in to unmask] Subject: [TN] component failures due to post wave/reflow washing Over the past years we have had relays, optos and pots fail due to corrosion being found inside the parts after post soldering wash. The quick solutions have been to use other manufacturer's parts or install after wash with hand solder "no-clean" cored flux. One manufacturer said it was because of halides in the flux. Our primary CM's and our flux contains halides, but we haven't seen as many failures with in-house processed PTH boards as with CM built boards. Recent pot failures have been explained by component manufacturers as too much wash pressure or bad flow direction from the wash jets. Opto failures were similarly diagnosed. Our in-house process, all PTH, is foam flux with OA flux, wave solder with 63/37 or SC995e followed by a closed loop DI wash with no chemicals. This has been a great process since 2006 when we switched from a no-clean foam flux, 63/37 wave and terpene/alcohol wash to our listed system above. We do not dictate flux/wash process to our CMs, but we do specify cleanliness to J-STD-001 C-22 using the 1.56 ėgm / cm2 NaCl equivalent contamination value. Forcing the CM to change fluxes for our product met great resistance and added cost so no change in flux was made. Our business is high voltage from 30 kV to 240 kV so clean with NO residue is very important. The DI wash has provided that in-house. We are using different CMs going forward, but not necessarily for this reason. Is this a problem unique to us or do other suffer from similar problems? Phil Nutting | HVP Development Engineer | Excelitas Technologies Corp Lab: +1 978.224.4332 | Office: +1 978.224.4152 35 Congress St, Salem, MA 01970 USA [log in to unmask]<mailto:[log in to unmask]> www.excelitas.com<http://www.excelitas.com/> [Description: Excelitas R_emailsig] Please consider the environment before printing this e-mail. ________________________________ This email message and any attachments are confidential and proprietary to Excelitas Technologies Corp. If you are not the intended recipient of this message, please inform the sender by replying to this email or sending a message to the sender and destroy the message and any attachments. Thank you. ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________