Hi all Let me give more details information. We found a few PCBA boards failed at our function test and the root cause is point to this BGA defective after our FAE debugged. We want to do some verification on these BGA. So we removed these BGA and re-balled these BGA. Then we re-mounted these re-balled BGA on fresh boards from SMT and go through our normal test process. These fresh boards with re-balled BGA still failed at our Function test. So we conducted these failed due to this BGA detective. So we want to send some samples to vendor for FA but unlucky we found pad missing of BGA after we removed. Lyon Yuan -----Original Message----- From: [log in to unmask] [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D. Sent: Thursday, September 05, 2013 12:29 AM To: [log in to unmask] Subject: Re: [TN] EXTERNAL: [TN] BGA pad drop Unless it was reballed and placed and soldered. The second heat cycle of removal may have caused the pad to come off. From: Bob Wettermann [mailto:[log in to unmask]] Sent: Wednesday, September 04, 2013 11:24 AM To: TechNet E-Mail Forum; Stadem, Richard D. Subject: Re: [TN] EXTERNAL: [TN] BGA pad drop Gents: Lyon wrote "Bob, After removed BGA, we found pad of BGA was missing." From what the patient is telling us it happened UPON REMOVAL (not during reballing process) Bob W On Wed, Sep 4, 2013 at 11:18 AM, Stadem, Richard D. <[log in to unmask]<mailto:[log in to unmask]>> wrote: I don't think so, as then the other pads would also display varying degrees of erosion. This appears to be a pad that was lifted during the reballing process, as part of the pad prep after rework (removal of the old solder). -----Original Message----- From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] On Behalf Of Gumpert, Ben Sent: Wednesday, September 04, 2013 9:20 AM To: [log in to unmask]<mailto:[log in to unmask]> Subject: Re: [TN] EXTERNAL: [TN] BGA pad drop Or potentially too much time at liquidus dissolved the pad away, or left minimal pad that was easily lifted. Ben -----Original Message----- From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] On Behalf Of Steve Gregory Sent: Wednesday, September 04, 2013 10:16 AM To: [log in to unmask]<mailto:[log in to unmask]> Subject: Re: [TN] EXTERNAL: [TN] BGA pad drop Well, well, well....there's your answer. I think someone did not have a delicate touch when they cleaned the pads... Steve -----Original Message----- From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] On Behalf Of Lyon Yuan Sent: Wednesday, September 4, 2013 8:14 AM To: [log in to unmask]<mailto:[log in to unmask]> Subject: Re: [TN] EXTERNAL: [TN] BGA pad drop Hi Steve Yes, it was re-balled Lyon Yuan From: stephen gregory [mailto:[log in to unmask]<mailto:[log in to unmask]>] Sent: Wednesday, September 04, 2013 10:11 PM To: Lyon Yuan; TechNet E-Mail Forum Subject: Re: [TN] EXTERNAL: [TN] BGA pad drop Hi Lyon! Have your picture posted, it's here: http://stevezeva.homestead.com/Pad_missing.JPG Do you know if this BGA was re-balled? Steve From: Lyon Yuan <[log in to unmask]<mailto:[log in to unmask]>> To: 'stephen gregory' <[log in to unmask]<mailto:[log in to unmask]>>; 'Steve Gregory' <[log in to unmask]<mailto:[log in to unmask]>> Sent: Wednesday, September 4, 2013 8:00 AM Subject: RE: [TN] EXTERNAL: [TN] BGA pad drop Steve, Help to upload picture to web. Thanks Lyon Yuan -----Original Message----- From: Wenger, George M. [Contractor] [mailto:[log in to unmask]<mailto:[log in to unmask]>] Sent: Wednesday, September 04, 2013 9:54 PM To: Lyon Yuan Cc: stephen gregory; Steve Gregory Subject: RE: [TN] EXTERNAL: [TN] BGA pad drop Lyon, Attached is a link to his site. The last emails I had for Steve are on the copy to line of this email <http://stevezeva.homestead.com/> http://stevezeva.homestead.com/ Regards, George George M. Wenger Failure Signature & Characterization Lab LLC 609 Cokesbury Road, High Bridge, NJ 08829 (908) 638-8771<tel:%28908%29%20638-8771> Home (732) 309-8964<tel:%28732%29%20309-8964> Mobile E-mail: <mailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]> <mailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]> -----Original Message----- From: Lyon Yuan [mailto:[log in to unmask]<mailto:[log in to unmask]>] Sent: Wednesday, September 04, 2013 9:45 AM To: Wenger, George M. [Contractor] Subject: RE: [TN] EXTERNAL: [TN] BGA pad drop George Thanks, steve's email? Lyon Yuan -----Original Message----- From: Wenger, George M. [Contractor] [mailto:[log in to unmask]<mailto:[log in to unmask]>] Sent: Wednesday, September 04, 2013 9:35 PM To: TechNet E-Mail Forum; Lyon Yuan Subject: RE: [TN] EXTERNAL: [TN] BGA pad drop Hi Lyon, You might want to send the picture to Steve to post on his site so we all can see it. Regards, George George M. Wenger Failure Signature & Characterization Lab LLC 609 Cokesbury Road, High Bridge, NJ 08829 (908) 638-8771<tel:%28908%29%20638-8771> Home (732) 309-8964<tel:%28732%29%20309-8964> Mobile E-mail: <mailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]> <mailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]> -----Original Message----- From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] On Behalf Of Lyon Yuan Sent: Wednesday, September 04, 2013 9:32 AM To: [log in to unmask]<mailto:[log in to unmask]> Subject: Re: [TN] EXTERNAL: [TN] BGA pad drop Hi Ben, I send a clear picture for your reference Lyon Yuan -----Original Message----- From: [log in to unmask]<mailto:[log in to unmask]> [mailto:[log in to unmask]<mailto:[log in to unmask]>] On Behalf Of Gumpert, Ben Sent: Wednesday, September 04, 2013 8:04 PM To: [log in to unmask]<mailto:[log in to unmask]> Subject: Re: [TN] EXTERNAL: [TN] BGA pad drop Lyon, I haven’t seen that. Typically the pads on the BGA are solder mask defined, which makes them much more secure than the usual non-solder mask defined pads on the PWB. Ben From: [log in to unmask]<mailto:[log in to unmask]> [mailto:[log in to unmask]<mailto:[log in to unmask]>] Sent: Wednesday, September 04, 2013 7:04 AM To: Gumpert, Ben Cc: TechNet Subject: Re:Re: [TN] EXTERNAL: [TN] BGA pad drop hi ben, it is pad missing from bga 在2013/09/04, "Gumpert, Ben" < <mailto:[log in to unmask]<mailto:[log in to unmask]>%3cmailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]><mailto:[log in to unmask]<mailto:[log in to unmask]>>> 写道: Lyon, By 'pad drop' do you mean lifted pads? (Pads stayed with the BGA?) Usually this means that there wasn't enough heat - that the solder was not melted in all locations. Ben -----Original Message----- From: TechNet <mailto:[mailto:[log in to unmask]<mailto:[log in to unmask]>]> [mailto:[log in to unmask]<mailto:[log in to unmask]>] On Behalf Of Lyon Yuan Sent: Wednesday, September 04, 2013 6:40 AM To: <mailto:[log in to unmask]<mailto:[log in to unmask]>%3cmailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]><mailto:[log in to unmask]<mailto:[log in to unmask]>> Subject: EXTERNAL: [TN] BGA pad drop guys,we found a few BGA pad drop after removed from pcba boards.what is reason to cause the issue ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or <mailto:[log in to unmask]<mailto:[log in to unmask]>%3cmailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]><mailto:[log in to unmask]<mailto:[log in to unmask]>> ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or <mailto:[log in to unmask]<mailto:[log in to unmask]>%3cmailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]><mailto:[log in to unmask]<mailto:[log in to unmask]>> ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or <mailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]> ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or <mailto:[log in to unmask]<mailto:[log in to unmask]>> [log in to unmask]<mailto:[log in to unmask]> ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask]<mailto:[log in to unmask]> ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask]<mailto:[log in to unmask]> ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask]<mailto:[log in to unmask]> ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask]<mailto:[log in to unmask]> ______________________________________________________________________ -- 1. Bob Wettermann 847-767-5745 ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________