John, I used to mold the specimen in well cured two-component Araldite, do the polishing with oil and diamond plastic discs to avoid contamination of the solder joint with polish particles. Use specimen rotating holder.Then wipe the stub with finest tissue to remove oil. Avoid solvents. Then perform a couple of minutes Argon sputtering, which will enhance the difference in hardness, Finally do microscopy with polarized light and a variable Nomarski lens, see page 119 here: http://bama.ua.edu/~mweaver/courses/MTE481/5_MTE481-MICROSCOPE&MODES.pdf There are many other methods of course, e.g. EDX element mapping mode, which I have practiced many a times. Inge On 21 March 2013 15:53, <[log in to unmask]> wrote: > What would a good etch be for etching SAC305 solder joints to enhance > viewing grain boundaries? > > Thanks, > John > > ______________________________**______________________________**__________ > This email has been scanned by the Symantec Email Security.cloud service. > For more information please contact helpdesk at x2960 or [log in to unmask] > **______________________________**__________ > ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________