I've always said "if someone's tougher than you, kick in the dipoles and they will bend over then". There is nothing wrong with the material. There are efforts to add an additive/filler that allows the dipoles to move when exposed to energy (force, thermal excursion approaching Tg) and be more flexible (change in modulus). There are many articles on pad cratering and ways to eliminate/minimize its effects. Before you go to that though make sure that's the problem. The best material in the world still needs to be properly drilled and plated to have a reliable interconnect strategy. Dewey -----Original Message----- From: Robert Kondner [mailto:[log in to unmask]] Sent: Wednesday, September 19, 2012 8:21 AM To: 'TechNet E-Mail Forum'; Whittaker, Dewey (EHCOE) Subject: RE: [TN] Broken Vias Dewey, Can you elaborate a little on the " this failure mechanism due to its inherent toughness"? I did notice literature showing that improper cure (too fast to hot) would cause the material to contract. I have seen that with epoxies in the past. Is this material schrikage the cause for the "Cratering" you were referring to? And if this is the case, over cure) what exactly is the nature of the failure? Thanks, Bob K. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Whittaker, Dewey (EHCOE) Sent: Wednesday, September 19, 2012 9:51 AM To: [log in to unmask] Subject: Re: [TN] Broken Vias Bob, 370HR is an excellent material and will pass the 6 cycles at 160ºC per IPC-TM-650, Method 2.6.27 with all three types of recommended via protection strategies, excluding the death slug (CB100). Are you sure the via failures are not pad cratering? This material with marginal designs is susceptible to this failure mechanism due to its inherent toughness (sorry for the dumbed-down technical term, I have been dealing with ISC). Dewey -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Robert Kondner Sent: Tuesday, September 18, 2012 5:38 PM To: [log in to unmask] Subject: [TN] Broken Vias Hi, This is a follow up on the broken vias on a board with plugged and plated through vias. The laminate is 370HR (Tg 180) and the fill material is PHP-900 IR-6P from San-Ei Kagaku (Tg 168). I do not have cross section pictures yet. If anyone has any ideas on how these material might react to a lead free reflow process and via barrels would be broken please let me know. I am interested in any and all ideas. Bob K. ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________