Best I can say going forward to answer the multiple questions below in one attempt, is that this is one of the reasons why we created IPC 9202 and rely on SIR testing, right. If it were as simple as merely deactivation of the activators, all No Clean Technical data sheets would supply a deactivation temperature, but last I looked most (if any) did not I'm not saying that reaching a perceived target temperature is not a good goal in order to minimize risk, but in a production environment, it is very difficult to depend that all topside residues have always meet this "sweet spot" temperature if it truly can be identified. What complicates the identification of this "sweet spot" is the other additives (surfactants, resins, co-solvents) added to liquids fluxes (especially) which can have a impact on what this deactivation temperature ultimately is and how it behaves. All kinds of other factors and synergisms come into play also with the specific process conditions and PCA components added to the mix. All my comments presented above, lets one answer questions such as "what is the proper deactivation temperature for my liquid flux?" with my all time favorite response.... "Well, it depends...". Rich Kraszewski (920)969-6075 -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo Sent: Monday, April 30, 2012 11:14 AM To: [log in to unmask] Subject: Re: [TN] 4 Questions: No Clean vs flux Deactivation. Possible Hogwash ??? Rich, Can you specify which formula? I am sure all the flux from different vendor are not made as per your claim "equal". Especially, it is not std requirements outlined as such: not reflowed flux shall pass SIR. I am looking forward to learn from you. Many thanks. Joyce Koo Materials Researcher - Materials Interconnect Lab Research In Motion Limited Office: (519) 888-7465 79945 Mobile: (226) 220-4760 -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Robert Kondner Sent: Monday, April 30, 2012 2:02 PM To: [log in to unmask] Subject: Re: [TN] 4 Questions: No Clean vs flux Deactivation. Possible Hogwash ??? Hi, If I read Rich correctly he is saying that flux formulated as No Clean is designed to pass the conditions specified on the data sheets without being "Thermally Deactivated". If that is correct it might be a "Big Time Wow" for a lot of folks on this list. Rich, Did I correctly summarize what you were saying? Thanks, Bob K. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Garcia, Rigo (GSFC-300.0)[MANTECH SRS TECHNOLOGIES] Sent: Monday, April 30, 2012 8:17 AM To: [log in to unmask] Subject: Re: [TN] 4 Questions: No Clean vs flux Deactivation. Possible Hogwash ??? Interesting input Rich. Are you then saying that in reality the activators don't ever get completely deactivated by the soldering process? Do we have to then, either rely on the encapsulating characteristics of the rosin/resin fluxes or rely on the cleaning process to get rid of them? Thanks for the feedback. Rigo Sr. Quality Assurance Engineer Workmanship Standards, Code 300 NASA, Goddard Space Flight Center Greenbelt, MD 20771 Phone. (301) 286-6129 Fax. (301) 286-6576 -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Richard Kraszewski Sent: Friday, April 27, 2012 5:18 PM To: [log in to unmask] Subject: Re: [TN] 4 Questions: No Clean vs flux Deactivation. Possible Hogwash ??? As a former flux formulator, we would never expect to rely on heat to deactivate (neuter) any flux activators. Reduce risk, sure. Eliminate, no. It was always part of good marketing and sales tool kit however, because it sounds plausible (& desirable). This kind of thinking related to thermal deactivation is not uncommon. Good example is the old Battelle Institute glutamic acid hydrochloride & urea concept. Heat releases the HCl for activity and the later & higher peak heat releases the urea activity to neutralize the free HCL. Was touted as ~a No-clean water soluble flux at one time. Actually worked rather well, but not enough to always count on the residues being harmless. Rich Kraszewski/PLEXUS -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Robert Kondner Sent: Thursday, April 26, 2012 9:45 AM To: [log in to unmask] Subject: [TN] 4 Questions: No Clean vs flux Deactivation. Possible Hogwash ??? Hi, 4 Questions (Please respond by number and elaborate if possible.) I have been listening to this thread about no clean fluxes and "Possible" problems with flux residues that have not been "De-Activated" through complete heating during a soldering process. First, I understand that a flux is "Activated", ie becomes chemically active, by heat. An example is ammonium chloride that when heated releases HCl (hydrochloric acid) which is a strong agent for cleaning a surface for good solderability. Below the temperature where a flux becomes "Activated" the flux in not active. IE: "All Cold Fluxes are De-Activated". Question 1: Are fluxes "Active" when they are cold? Is a RMA active when it is cold? If the above is true what is all the stuff about "Active Flux" remaining on a PCB surface? Hogwash? Further, I know from experience that reflow temperatures that are too high or too long "Burn Off" the flux and provide very poor surface finishes. If so this implies a significant portion of un-used flux will remain on the PCB after the reflow cycle. Flux will not be "Activated" once the PCB cools but it will remain active during the liquid solder phases. Question 2: Is it true that we want flux active throughout the entire liquid solder phase and does this imply there should be un-altered flux remaining on the PCB surface after the reflow period? (Me Thinks Yes?) A good example is an RMA flux. From experience I know RMA fluxes have a very wide processing window, You can "Touch Up" a joint covered with RMA without additional flux because of RMA robustness. It simply leaves a "Messy" board finish. Also, it has been my understanding that leaving an RMA flux on a PCB was a "Cosmetic Issue" but I do find that hard to believe. There must be "Bad Stuff" in all that gunk left behind. But wire solder and RMA flux has been used for decades and is considered "OK" to remain on a PCB, I think. Question 3: Are any flux chemistries acceptable to be left on a PCB and not cleaned and would such PCBs pass an ionic contamination test? Question 4: Do all the companies that make "No Clean" Flux lie when they call them "No-Clean"? Thanks, Bob K. > I have an issue with one of the assembly houses we use. They are > using a No-clean flux that contains adipit and succinic acids (per the > MSDS) in an alcohol base. > > Is it allowed to leave flux on the PWB that HAS NOT BEEN DEACTIVATED > BY HIGH TEMPERATURES OF SOLDERING? > > I am not talking about the flux used in the solder paste or wave > soldered flus. I am talking about the flux used at rework and > touch-up of the PWB. > > ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------------------------- This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful. ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________