Thank you Andy, I wouldn't "worry" much about which phase is "going farther", as it the phases have different viscosity, but rather about the wetting angle. I should probably give you some of the background to my original question. We got a component after re-flow (Pb-Sn solder, but some of the Au-finished terminations were not soldered). What I saw with EDS was that part of those unsoldered terminations has relatively half of the area intact (still covered with Au), while the rest is covered with a thin layer (comparable to the original Au layer) of Pb--rich film. I thought that if Pb-rich phase has a lower wetting angle, compared to the Sn-rich one, it could give me a clue on what could have happened. Vladimir SENTEC Testing Laboratory Inc. 11 Canadian Road, Unit 7. Scarborough, ON M1R 5G1 Tel: (416) 899-1882 Fax: (905) 882-8812 www.sentec.ca -----Original Message----- From: "Giamis, Andy" <[log in to unmask]> Sender: TechNet <[log in to unmask]> Date: Fri, 13 Apr 2012 13:21:59 To: <[log in to unmask]> Reply-To: TechNet E-Mail Forum <[log in to unmask]>, "Giamis, Andy" <[log in to unmask]> Subject: Re: [TN] Wetting angles Vladimir, I refer to Sn-rich and Pb-rich phases in eutectic SnPb. In cross-section showing a contact angle, the Sn-rich phase always leads the Pb-rich phase. SnPb wets very well to Au or Ag. If we eliminate any capillary action (as in solder flowing between plates), the leading edge of the Sn-phase on polished Au or Ag can approach zero - certainly below 5 degrees. If you add surface roughness, contamination, dust, oxides, or anything else, then the angle grows. A simple measurement would be to take an Au-plated bare board, put it on a hot plate and lightly drop some very small drops of molten SnPb solder onto the surface. If you are delicate and produce small drops (perhaps about 5 mm across, you should be able to assume spherical caps. Measure the diameter and height of the drop. From that, you can calculate contact angles for your surface. I've done this with flip-chip underfills. It works remarkably well. Regards, Andy Andrew C. Giamis Andrew Solutions FMA / Reliability Engineer 40 Technology Drive, Warren, NJ 07059 (908) 546-4686 [Office] (908) 938-7945 [Cell] [log in to unmask] -----Original Message----- From: vladimir Igoshev [mailto:[log in to unmask]] Sent: Friday, April 13, 2012 1:30 PM To: Giamis, Andy; [log in to unmask] Subject: Re: [TN] Wetting angles Thank you Andy, Two questions, though. Do you know the actual values, as they should be far higher than 0 (it's not liquid He we are talking about :-)). Secondly, do you refer to pure Pb and Sn or Pb-rich and Sn-rich phases? ------Original Message------ From: Giamis, Andy To: [log in to unmask] To: [log in to unmask] Subject: RE: [TN] Wetting angles Sent: Apr 13, 2012 12:47 Typically the Sn phase wets out farther than the Pb phase. On a good clean Au surface, the contact angle approaches zero. Regards, Andy Andrew C. Giamis Andrew Solutions FMA / Reliability Engineer 40 Technology Drive, Warren, NJ 07059 (908) 546-4686 [Office] (908) 938-7945 [Cell] [log in to unmask] -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of vladimir Igoshev Sent: Friday, April 13, 2012 12:43 PM To: [log in to unmask] Subject: [TN] Wetting angles Technetters, I have a simple question. Does anyone know what the wetting angles of the two phases of the Pb-Sn eutectic on a Au surface are. Or at least which one is lower? Any direct answer (number/reference) will be greatly appreciated. Regards, Vladimir SENTEC Testing Laboratory Inc. 11 Canadian Road, Unit 7. Scarborough, ON M1R 5G1 Tel: (416) 899-1882 Fax: (905) 882-8812 www.sentec.ca ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ Vladimir SENTEC Testing Laboratory Inc. 11 Canadian Road, Unit 7. Scarborough, ON M1R 5G1 Tel: (416) 899-1882 Fax: (905) 882-8812 www.sentec.ca ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ ______________________________________________________________________ This email has been scanned by the Symantec Email Security.cloud service. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________