Bob, Thanks for the prompt support. Some more info : On failed PWA, the communication between SDRAM and FLASH stops at -20oC. The units boots and hang or just refuses to boot. Once temperature reaches back -10oC, the unit operates again. Dye&pry showed potential poor joints on the balls but nothing conclusive. We conducted EDX on both failed PWA and fresh PCB. Both showed P-content 0.5% above IPC specs. Black-pad originates from high Phosphorous content. But, how severe is 10.4%wt P-content ? Regards, Fabien From: Bob METCALF [mailto:[log in to unmask]] Sent: Tuesday, October 18, 2011 10:07 To: TechNet E-Mail Forum; Fabien Guizelin Cc: [log in to unmask] Subject: Re: [TN] High Phosphorous content on ENIG PCB Fabien, It would be helpful to understand the nature of the failure. You mention it was a low temp failure. I don't understand what the failure is. Could you please expand on this? As far as the P content being slightly about 10%, assuming it is a mid to high phos nickel, I wouldn't expect a problem, but not knowing what has failed it would be difficult to speculate. Regards, Bob Metcalf Western Regional Manager Atotech USA Inc 1750 Overview Drive Rock Hill, South Carolina 29730 USA Mobile: 714-334-7667 e-mail: [log in to unmask] Internet: www.atotech.com<http://www.atotech.com/> Managing Director: Kuldip Johal This e-mail and any attachments hereto are business documents of Atotech USA Inc. and may contain CONFIDENTIAL OR PROPRIETARY BUSINESS INFORMATION. Unauthorized disclosure and/or use of information contained in this e-mail are prohibited. If you are not the intended recipient, you should dispose of it and not use, disseminate or copy this message or any other files transmitted with it. [cid:[log in to unmask]] . From: Fabien Guizelin <[log in to unmask]> To: <[log in to unmask]> Date: 10/17/2011 05:42 PM Subject: [TN] High Phosphorous content on ENIG PCB Sent by: TechNet <[log in to unmask]> ________________________________ Hi all, I am facing a PWA failure at low temperature. An EDX analysis revealed a P-content of 10.4%wt which is outside the IPC-4552 1.2.1 specifications (7-10%). The PCB has an ENIG finish. Could I be facing black-pad ? How severe is the 0.4%wt additional Phosphorous content ? Regards, Fabien ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------