I would recommend that you do dry bake them at say 120 deg for at least an hour to dry out the PCB, the other option would be using a moisture absorbing chemical. We have recently repaired a bunch of 40 year old single sided boards, measling was an issue due to the moisture content of the boards. We did heat the ones that required extensive rework with a heat gun for a few minutes and that helped. However I prefer to put them in our environmental oven for at least 4 hours to dry them. Pat Goodyear Control tech PG&E -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Joe Macko Sent: Tuesday, June 07, 2011 10:48 AM To: [log in to unmask] Subject: [TN] PCB dry-bake requirement for thru hole connector replacement All, I would like to hear some comments as well as lessons learned from the experts concerning the basic requirement to dry-bake populated boards prior to some thru hole connector replacement. The boards are double sided and are also populated with numerous SMT components, some of which are moisture sensitive. Solder alloy is SnPb. Our normal process is to dry-bake "PCBs" prior to reflow and so the question came up if we should also dry-bake the now populated boards prior to replacement of some thru hole connectors to prevent potential damage to the PCB and/or surrounding parts. The connectors will be removed and replaced using either one or a combination of a Selective Solder machine and\or solder pot. If we were doing a BGA replacement using a hot air machine, we would dry-bake the populated board. Thanks again for the valuable feedback. -Joe "This e-mail and any attachments are solely for the use of the addressee and may contain L-3 proprietary information that may also be defined as U.S. Government export controlled technical data. If you are an unintended recipient of this e-mail, use, disclosure or distribution of its content is prohibited. Please notify the sender by return e-mail and immediately delete this message." ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------