I just can't but help add a few comments. Based on thermal cycle testing finish has a PWB reliability role. In very few words. Any finish using heat may degrade copper and dielectric reliability. Lead free finishes are more degrading than tin lead finishes. I am beginning to think fused tin/lead may be the most degrading surface finish. Any finish with nickel tends to extend cycles to failure by stopping barrel cracks, protecting PTH barrels. If internal interconnections are weak nickel may enhance the degradation of internal interconnection reducing cycles to failure. Generally nickel greatly extends cycles to failure but poorly applied, nickel with skips, nicks or bubbles in the PTH may reduce cycles to failure by 2/3. Best regards, Paul Reid _____ From: TechNet on behalf of Joyce Koo Sent: Thu 02/06/2011 1:18 PM To: [log in to unmask] Subject: Re: [TN] Best Board Finish - beyond gold It depends. Some HASL are really flat. It is all vendor dependent. Want HASL with super clean (no trapped oil, glycol, etc), low IMC, flat and cheap, is hard to get. -------------------------- Sent using BlackBerry ----- Original Message ----- From: Post, Scott E [mailto:[log in to unmask]] Sent: Thursday, June 02, 2011 12:33 PM To: [log in to unmask] <[log in to unmask]> Subject: Re: [TN] Best Board Finish - beyond gold It can be really difficult to get solder paste to release consistently on very fine features with HASL. Also, the domed shape of HASL can cause poor stencil gasketing that leads to solder squeezing down the sides of the land and bridging. Every company seems to have a different threshold where they won't use HASL. I know some people won't use it on boards that have 0402s and 0.5 mm pitch QFPs. I personally think HASL is OK for those feature sizes but below that causes too much grief. In fact, last month I ran an experiment using a board design with 0.4 mm pitch QFPs and BGAs as well as some resistor arrays with very fine apertures. I had the same board design with OSP and SN100 HASL. The difference in print quality was dramatic even though the HASL boards had what I consider very good HASL. I'd hate to think how bad the print quality would have been with some of the variation we see in Pb free HASL quality. Scott Post Staff Manufacturing Engineer P.O.U. 0000-001E-0CTC 2151 E. Lincoln Road Kokomo, Indiana 46904-9005 765-451-2983 (Phone) 765-451-0287 (FAX) -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Robert Kondner Sent: Thursday, June 02, 2011 11:37 AM To: [log in to unmask] Subject: Re: [TN] Best Board Finish - beyond gold Bob, As for flatness: once a PCB has paste printed can you even tell what the finish is? I have never been able to figure out this flatness thing. As for reliability I think solderability wins every time. Are you telling me these other finishes have better solderability than, well solder, as found only in a HASL finish? Has anyone ever seen "Black Pad" with HASL? There is no Ni so the P cannot be wrong, ever. Right? I fell like a stick in the mud on my bias towards HASL, I am open to ideas here. Bob K. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Bob METCALF Sent: Thursday, June 02, 2011 11:18 AM To: [log in to unmask] Subject: Re: [TN] Best Board Finish - beyond gold When considering finishes, if the ultimate in reliability and surface flatness are key considerations, you must give electroless nickel, electroless palladium, immersion gold (ENEPIG) some consideration. Regards, Bob Metcalf Western Regional Manager Atotech USA Inc 1750 Overview Drive Rock Hill, South Carolina 29730 USA Mobile: 714-334-7667 e-mail: [log in to unmask] Internet: www.atotech.com Managing Director: Kuldip Johal This e-mail and any attachments hereto are business documents of Atotech USA Inc. and may contain CONFIDENTIAL OR PROPRIETARY BUSINESS INFORMATION. Unauthorized disclosure and/or use of information contained in this e-mail are prohibited. If you are not the intended recipient, you should dispose of it and not use, disseminate or copy this message or any other files transmitted with it. . From: "Stadem, Richard D." <[log in to unmask]> To: <[log in to unmask]> Date: 06/02/2011 07:46 AM Subject: Re: [TN] Best Board Finish - beyond gold Sent by: TechNet <[log in to unmask]> I agree with everything you say, Barbara. It sounds like you are now on your way to making the correct choice. Stay away from immersion tin. If you choose immersion silver, refer to both IPC 1601 and IPC 4553 for storage and handling considerations. They can be managed. The double-sided process can leave a slight reduction of solderability with immersion silver PWBs by the time you are ready to hand solder any PTH parts, making that more difficult to do, sometimes. That is why I asked. Also, if you select Immersion Silver, make sure that your PWB fabricator has a good plating product, a well controlled process and some experience with it. Ditto with ENIG. Especially with ENIG. Regarding immersion silver, it is susceptible to environments that are heavy in sulfides, such as automotive exhaust, rubber processing, or paper processing. Keep some of these things in mind both from an end-use environment standpoint and from a storage standpoint. Do not store in areas where there are open containers of soaps, fluxes, etc., nearby. From: Barbara Burcham [mailto:[log in to unmask]] Sent: Thursday, June 02, 2011 9:22 AM To: Stadem, Richard D. Cc: TechNet E-Mail Forum Subject: Re: [TN] Best Board Finish - beyond gold Thanks everyone for you imput. What a great group of people! Richard, The application will be double sided, fine pitch array components, some through hole components and going into a shock environment. I will need to connect with the assemblers to check on flux and paste compounds. Does this information help? You make an excellent point. Must have the total picture. I do not know, yet, how long boards will sit on the shelf before moving into assembly, either. I do know that shelf life will also impact this decision. I do not think that I want to use tin...that hairy growth stuff. Barbara On Thu, Jun 2, 2011 at 8:01 AM, Stadem, Richard D. <[log in to unmask]< mailto:[log in to unmask]>> wrote: Barbara, What is the application, board type, component types, etc? Immersion silver is my personal favorite, but that is completely irrelevant. You should choose a board finish dependent upon the application of the CCA, whether it has fine-pitch array components, including CSPs, whether it is double-sided with PTH parts or hand-soldered components, the environment the CCA will be used in, the flux type to be used, the alloy that is required, and several other factors that go into the decision. Without complete knowledge of all these factors, it is hard for anyone to answer that question. I can tell you that IAg beats ENIG in cost, but each finish has strengths and weaknesses. Some definitely have more or less than others. -----Original Message----- From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] On Behalf Of Barbara Burcham Sent: Wednesday, June 01, 2011 8:17 PM To: [log in to unmask]<mailto:[log in to unmask]> Subject: [TN] Best Board Finish - beyond gold Hey Y'all, I am looking for a reliable bare board finish that beats the cost of gold. What experience is out there? What would you recommend? Thanks, Barbara Burcham pcb Trace Design [log in to unmask]<mailto:[log in to unmask]> ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask]< mailto:[log in to unmask]> ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask]<mailto:[log in to unmask] > with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask]< mailto:[log in to unmask]> or 847-615-7100 ext.2815<tel:847-615-7100%20ext.2815> ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- **************************************************************************************** Note: If the reader of this message is not the intended recipient, or an employee or agent responsible for delivering this message to the intended recipient, you are hereby notified that any dissemination, distribution or copying of this communication is strictly prohibited. If you have received this communication in error, please notify us immediately by replying to the message and deleting it from your computer. Thank you. **************************************************************************************** ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------------------------- This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful. ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 16.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------