I see a fairly large piece of string or thread and two inspection arrows in the solder in the pictures. It may be time to clean the solder pot thoroughly. Items such as string, labels, etc, will not show up in the pot analysis, as that analysis is typically only for various metal alloys (tin, antimony, indium, bismuth, lead, gold, silver, etc.) However, the analysis should be done first to help determine just what should be done with the solder in the pot. You may need to thoroughly clean out all the dross and flux lining the inside walls of the sump and then just add tin to get it slightly above 63%, or it may be so contaminated with other alloys that you may need to take out all or most of the old solder, clean the sump, and replace with fresh solder. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory Sent: Monday, January 17, 2011 2:56 PM To: [log in to unmask] Subject: Re: [TN] Board failure due to fibber like fragments of alloy after wave soldering Hi Cedric, What does your last solder analysis say? You do get your pot analyzed don't you? Steve **** From: TechNet [mailto:[log in to unmask]] On Behalf Of Cedric ORAIN Sent: Monday, January 17, 2011 2:57 PM To: [log in to unmask] Subject: [TN] Board failure due to fibber like fragments of alloy after wave soldering After wave soldering of boards with both SMD and PTH components, 18% of the boards failed during ICT. The failure is due to shorts between SMD pads. These shorts are caused by "fibber like" fragments entrapped in solder joints. We are looking for root cause of this level of waste. These fragments are very similar in aspect with dross that we found on the top of the wave "head" after the pump stop. You can see dross picture in the pictures posted here: http://ipc-technet.groupsite.com/gallery/17663 The alloy is Sn63Pb37 and the flux is an alcohol based no-clean flux. Soldering under air atmosphere. The design of the board is ok. Dross is removed daily. Did you ever encountered this kind of issue (I mean with such a rate of defect)? I'm wondering if the aspect of the dross shown in the picture is normal or is it due to a pollution (metallic pollution: high Cu rate?? / organic pollution : epoxy, fiber glass fragments ...). Thanks for your in advance for your help and support, Best regards, Cedric ORAIN ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------