My experience has been that usually only the BGA pads will exhibit fractures associated with BP. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Phil Bavaro Sent: Tuesday, October 12, 2010 12:07 PM To: [log in to unmask] Subject: Re: [TN] Mech. damage or poor wetting? Thus.....etc I would want to inspect the rest of the board for more evidence of the black pad, such as the smaller chip caps....for it to only occur at the perimeter of the bga seems unlikely. On a chip cap pad which has had solderpaste melt and interact with the nickel underneath, the dewetting should be apparent. Dye and Pry can be misleading as to the cause of the dye penetration, especially when there are numerous possible mechanical questions. Phil -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D. Sent: Tuesday, October 12, 2010 9:40 AM To: [log in to unmask] Subject: Re: [TN] Mech. damage or poor wetting? It sure looks like Black Pad to me. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor Hernandez Sent: Monday, October 11, 2010 2:41 PM To: [log in to unmask] Subject: Re: [TN] Mech. damage or poor wetting? Was this BGA reworked/repaired. Is it in close proximity to another BGA that was RW? Did the card/board see two consecutive thermal excursions? X" -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Thayer, Wayne - IIW Sent: Monday, October 11, 2010 1:55 PM To: [log in to unmask] Subject: Re: [TN] Mech. damage or poor wetting? Never mind. I just read the original post. I'm betting the whole shebang is due to poor wetting--that's why the correlation to the fanout escape. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Thayer, Wayne - IIW Sent: Monday, October 11, 2010 2:52 PM To: [log in to unmask] Subject: Re: [TN] Mech. damage or poor wetting? What's going on with the picture of the cross section? The ball isn't wetting down the side of the plated pad. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Chris Mahanna Sent: Monday, October 11, 2010 2:41 PM To: [log in to unmask] Subject: Re: [TN] Mech. damage or poor wetting? Here are a few pictures http://ipc-technet.groupsite.com/gallery/16011 this job is a mixed bag. Currently we suspect soldering, cratering, ICT and t-cycling damage Chris From: [log in to unmask] [mailto:[log in to unmask]] Sent: Monday, October 11, 2010 2:22 PM To: TechNet E-Mail Forum; Chris Mahanna Cc: [log in to unmask] Subject: Re: [TN] Mech. damage or poor wetting? Hi Chris - do you have any pictures you can share? Dave Hillman Rockwell Collins [log in to unmask] Chris Mahanna <[log in to unmask]> Sent by: TechNet <[log in to unmask]> 10/11/2010 11:29 AM Please respond to TechNet E-Mail Forum <[log in to unmask]>; Please respond to Chris Mahanna <[log in to unmask]> To [log in to unmask] cc Subject [TN] Mech. damage or poor wetting? We have a BGA dye-n-pry job that shows board side sj damage with a strong correlation to fan-out clocking. We also have some microsection evidence of poor wetting. All damage/dye is on perimeters. Is this an indication of heat sinking and subpar wetting, or can it be completely mechanical? Both? Thanks Chris ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- This e-mail and any files transmitted with it may be proprietary and are intended solely for the use of the individual or entity to whom they are addressed. If you have received this e-mail in error please notify the sender. Please note that any views or opinions presented in this e-mail are solely those of the author and do not necessarily represent those of ITT Corporation. The recipient should check this e-mail and any attachments for the presence of viruses. ITT accepts no liability for any damage caused by any virus transmitted by this e-mail. ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------