Richard, I beg to differ... This assumes you have perfectly clean components, PCB and printing system... If the connection elements have removable surface metallic compounds, the PCBs have ionics or contamination on them and the stencil and blade are contaminated, all of these will be entrapped by the no-clean flux when it "cures" in reflow...Since the flux residue is hydroscopic all the contaminates will sit in the flux matrix until sufficient moisture and/or temperature occurs to induce a conditionally conductive matrix... If I remember correctly the use of no-cleans was more due to economic drivers not performance... Thus the economics of the product becomes the criteria for its use and environmental reliability testing data is the justification... Paul Paul Edwards Surface Art Engineering -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D. Sent: Wednesday, October 20, 2010 8:06 AM To: [log in to unmask] Subject: Re: [TN] Cleanable Long Stencil Time Flux Question Hold on, Bob. Bad info. No-clean flux residues from solder paste ARE inerted when they go through reflow. Most of the issues with no-clean flux are for benchtop liquid flux applications during rework or hand-soldering, which may not be fully inerted because the heat from a solder iron tip is not sufficient to do so, and because the liquid tends to run under places it was not intended to go. However, careful application of no-clean liquid fluxes using a felt-tip dispenser with a good operator are usually pretty safe. No-clean solder pastes are used daily on circuit boards by the million, with few or no issues. While not favored for military or high-rel use, they work well in many other applications. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Bob Landman Sent: Wednesday, October 20, 2010 9:51 AM To: [log in to unmask] Subject: Re: [TN] Cleanable Long Stencil Time Flux Question Bob K, I'm sure this will ignite a debate but personally, I wouldn't allow any of our boards to be assembled with "no-clean" solder paste. Perhaps Terry Munson can share with you some photos of why that's a bad idea. Not all the flux is inerted by the reflow process, so I'm advised. Check out his website at http://residues.com/ This paper should give you some ideas http://residues.com/pdfs/Circuits%20Assembly%20Articles/2004/low%20res/2004.03-The%20Key%20to%20Success%20-%20Circuits%20Assembly.pdf Also this one http://residues.com/pdfs/Circuits%20Assembly%20Articles/2003/low%20res/2003.03-Component%20Cleanliness%20in%20a%20No-Clean%20World%20-%20Circuits%20Assembly.pdf I've visited Terry's facility in Kokomo, IN. He's got an incredible array of diagnostic instrumentation, some of which he has designed and manufactured himself (like the C3). Bob Landman H&L Instruments, LLC -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Robert Kondner Sent: Wednesday, October 20, 2010 10:10 AM To: [log in to unmask] Subject: [TN] Cleanable Long Stencil Time Flux Question Can anyone make a paste/flux suggestion? In a past life I once used a No Clean Alpha Metal 6106 paste which had an incredibly long stencil life, I think it was 8 hours. This stuff never really "Dried Out" and a pasted board could sit for two days and a "Missing Part" could thus be ordered and reflow soldered. Trouble was NOTHING would remove this no clean flux and trying to wash messy THT or Rework flux could make a real mess. Can anyone suggest a cleanable paste/flux that has a long stencil life and does not dry out to a hard crust? Thanks, Bob K. ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ============================================================================== This email and any attachments thereto may contain private, confidential, and privileged material for the sole use of the intended recipient. Any review, copying, or distribution of this email (or any attachments thereto) by others is strictly prohibited. If you are not the intended recipient, please contact [log in to unmask] immediately and permanently delete the original and any copies of this email and any attachments thereto. ============================================================================== ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------