I was going to say, my understanding of the P addition was to modify the grain/plated properties of the NI, to give good mechanical properties rather than directly as a solderability control, but Werner's answer covers that and rather more! As is his norm. There are proprietary "solderable" Ni plates. Solderable meaning less readily/more slowly passivating, but these are more usually employed on structural assemblies like large heat sinks, packages rather than PCB finishes. For regular PCB finishes the N is protected to maintain solderability with thin Au - to give us ENIG, or sometimes Ag or even Sn. [I personally do not consider that Pd containing finishes protect or improve solderability.] Regards Mike -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier Sent: Tuesday, September 21, 2010 3:40 PM To: [log in to unmask] Subject: Re: [TN] Solderability of nickel plating Hi Kevin, Now my 5 cents. From my experience, I do not see solderability directly linked to the concentration of phosphorus co-plated with the nickel-I see however, brittle interfacial failures between the Ni-P surface and the Ni3Sn4-intermetallic compound which directly track with P-concentration at that interface. The presence of Ni3Sn4-IMC is clear evidence that there was no solderability issue-it is the concentration of the P at the interface which weakens the interfacial bond. Because of their superficial appearance, conditions with both too much P and too little P [causes hyper-galvanic corrosion along the grain boundaries of the Ni plating] have been termed 'black pad.' Having too much P at the interface can be the result of improper Ni-plating, but also the result of too much Ni being dissolved in the Sn of the solder leaving to much P behind-this can happen from too many soldering operations. Werner -----Original Message----- From: Glidden, Kevin <[log in to unmask]> To: [log in to unmask] Sent: Tue, Sep 21, 2010 8:52 am Subject: [TN] Solderability of nickel plating All, Can anyone comment on the solderability of the nickel plate, particularly with regard to type of plating: high phosphor / low phosphor, and also storage conditions: I've been gathering info, and seen conflicting information. From one article: http://corrosion-doctors.org/MetalCoatings/Electroless.htm A paper submitted at the Electroless Nickel conference of 1989 held in Cincinnati Ohio, Titled "Solderability Parameters of Elecroless Nickel Bearing Electronic Finishes" By Louis Kosarek of STB Systems, Inc. report that "An electroless nickel deposit which contains a concentration of phosphorus ranging from 0.1% to 3.0% is readily solderable on an "As-plated Basis" per Mil-Std 883c method 2003. The frequency of solderability tests which fail per Mil-Std 883c will increase as the phosphorus content of electroless nickel alloy increases from 3.0 to 7.0% phosphorus. A solderability test conducted per Mil-Std 883c method 2003 incorporating an as-plated surface finish containing phosphorus in excess of 7%, the components will consistently fail. The mode of failure is non-wetting of the surface." This indicates low phosphorous plating is best for solderability. Many other papers seem to agree with this. ---------------------------------------------------------------------------- ----------------------------------------- From another article: http://www.pfonline.com/articles/pfd0024.html Solderability/Weldability. An important aspect of electroless nickel to the electronics industry is its solderability. All electroless nickel deposits are solderable provided the soldering conditions are matched to the condition of the particular electroless nickel deposit. Lower-phosphorus electroless nickel is more easily solderable immediately after plating than higher-phosphorus electroless nickel. However, this advantage disappears after 12 - 24 hrs. At this point, the ease of solderability depends upon the characteristics of the passive layer that forms on the surface of the electroless nickel deposit. Those deposits plated from baths containing heavy metal and sulfur-bearing brighteners and stabilizers, such as most commercial low- and mid-phosphorus electroless nickel systems, form a thicker tenacious passive layer than those that do not, such as most high-phosphorus electroless nickel systems. High-phosphorus electroless nickel systems tend to be more solderable in aged deposits. Other important factors influencing the solderability of electroless nickel deposits include residual contamination left on the surface after plating and storage conditions after drying. Surface contamination and exposure to environments containing sulfur dioxide, chlorine, high humidity and high ambient temperatures will detrimentally affect solderability. Therefore, it is imperative that parts be thoroughly rinsed in clean DI water, dried and stored in a cool, dry atmosphere, preferably nitrogen. This article indicates high phosphorous plating is best for long term solderability, and also that parts must be stored carefully (cool, dry, sealed, nitrogen). Other articles seem to state this is a highly stable finish and is even used as a corrosion inhibitor. Thanks, Kevin Glidden Manufacturing Engineer Astronics Luminescent Systems Inc.<http://www.astronics.com> 4 Lucent Drive Lebanon, NH 03766 (603) 643-7766 x3152 Please note, LSI operates on a 9/80 work schedule, and is closed on alternating Fridays. Please click the link provided to view the days LSI will be closed. http://www.astronics.com/LSI/documents/2010calendar-NH.pdf NOTICE: This communication is intended specifically for the recipient(s) named above and may include proprietary, confidential or privileged information. If you are not a named recipient, you should immediately delete or destroy all electronic and physical copies of this communication. Unintended recipients also should not utilize, repeat, publish or relay to any other person the information contained herein nor should they take any action based upon, in whole or in part, such information. If you have received this message in error, you are requested to contact the sender immediately. EXPORT COMPLIANCE STATEMENT: The information contained herein is or may be controlled by the International Traffic in Arms Regulations (ITAR), 22 CFR 120-130, or the Export Administration Regulations (EAR) and may not be exported, or disclosed to a foreign person, whether in the United States or abroad, without prior U.S. Government and Astronics Luminescent Systems written approval. Violations of these regulations could result in administrative, civil or criminal penalties. If you have any questions about the nature of the material contained in this email please contact the sender immediately. ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ***This email, its content, and any files transmitted with it, are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient, please contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination, or other use of, or taking of any action in reliance upon this information by persons or entities other than the intended recipient is prohibited. Messages sent via this medium may be subjected to delays, non-delivery, and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. Indium Corporation does not accept responsibility for changes made to this email after it was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.*** ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------