Any additional data on this would be great. I have been pushing this finish for several years. This way they won't be thinking I'm trying to sell them an ENEPIG in a poke. Dewey -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman Sent: Thursday, August 26, 2010 6:58 AM To: [log in to unmask] Subject: Re: [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT PARTS Hi George - no rush on finding the report. If there are no release restrictions we could possibly put it on the IPC web page or have Steve post it on his web page. The data in that report would be of interest to many TechNet folks. Dave "Wenger, George M." <[log in to unmask]> 08/26/2010 08:56 AM To TechNet E-Mail Forum <[log in to unmask]>, "[log in to unmask]" <[log in to unmask]> cc Subject RE: [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT PARTS Hi Dave, It didn't get published in a conference but give me 24 hours to go through my old records and I may be able to find the NCMS Summary report put out at the end of the 5 year project and I'll send it to you. I'd look for it right now but I've got a couple of crisis situations (work related) I'm addressing and as luck would have it my management also wants me to interview two candidates today. Regards, George George M. Wenger Andrew Solutions Senior Principal FMA/Reliability Engineer 40 Technology Drive, Warren, NJ 07059 (908) 546-4531 (Office) (732) 309-8964 (cell) [log in to unmask] -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman Sent: Thursday, August 26, 2010 9:43 AM To: [log in to unmask] Subject: Re: [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT PARTS Hi George - excellent information! I didn't realize the overall cost savings on the component fab process was that extensive. You also reminded me that there was a large NCMS printed wiring boards surface finish consortium effort in the late 80s (?) which you, Jim Reed of TI , and others participated in which produced some very good early data on the impact of Pd as a potential pwb surface finish. Some of the Pd embrittlement and solderability shelf life data used by the industry came out of the work that you conducted. Some of that data was published at the IPC Surface Finishes Conferences. Did it get published elsewhere? Dave "Wenger, George M." <[log in to unmask]> 08/26/2010 08:34 AM To "[log in to unmask]" <[log in to unmask]> cc Subject RE: [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT PARTS Dave, You knowledge of the PdNiAu history is similar to mine.I'd go one step further and say that TI pushed PdNi because it was a big cost saving, except for the period when Pd prices skyrocketed. Using pre-plated PdNi lead frames allows them to eliminate post-molded lead plating and in the time period when they introduced PdNi SnPb plating had been the standard lead plating so the big saving to them was not having to handle Pb effluent in spend plating baths. So they eliminated the cost of the plating chemicals , the cost of the plating process, and the cost associated with disposal of spent plating chemistry. The addition of Au to PdNi came about because several of us who were using TI PdNi components found that components in inventor were losing their solderability because, as you said, the Pd is a good catalyst material and pulls stuff out of the air. So their response was to put Au on the Pd to protect the Pd rather than as an added protection for the Ni. Regards, George George M. Wenger Senior Principal FMA / Reliability Engineer Andrew Corporation - Wireless Network Solutions 40 Technology Drive, Warren, NJ 07059 (908) 546-4531 Office (732) 309-8964 Mobile E-mail: [log in to unmask] -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman Sent: Thursday, August 26, 2010 8:28 AM To: [log in to unmask] Subject: Re: [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT PARTS Hi Inge - the history of the Ni/Pd/Au plating stackup is kinda interesting. There has been lots of industry Pd plating soldering and wirebonding investigations during the last 50 years. The work that has always caught my attention was the published data in the late 1980s and early 1990s. Texas Instruments investigated the use of Ni/Pd plating as a substitute material for component leadframe spot silver process which was part of the component wirebonding protocol. I was told that using Ni/Pd provided both some technical and process advantages. Texas Instruments patented the Ni/Pd plating concept (in terms of component applications) and then implemented the concept on their component processes. The whole concept was almost wiped out as the price of Pd skyrocketed (4X-5X price increases per troy ounce) for a couple of years as a couple of countries (Russia and South Africa were the rumored conspirators) locked up their Pd stockpiles and messed up the global market. The insanity passed and things went back to normal. Texas Instruments amended its patent to include a flash gold to seal off the Pd from the environment degradation (Pd is a good catalyst material so it tended to react with some storage environments resulting in a loss of solderability). The Pd layer is not very thick as you can get Pd embrittlement in a similar fashion to Au embrittlement. As Richard detailed, we are really soldering to the Ni plating with the Pd and Au being oxidation protectors of the Ni surface. In the early 2000s, the RoHS actions began and since Ni/Pd/Au doesn't create tin whiskers, life suddenly became very good for the surface finish. Additionally, the industry interest in ENEPIG is another extension of the industry assessing Pd, in combination with Ni and Au, for both soldering and wirebonding characteristics. It appears that the industry fascination with Pd is going to be a topic of interest for quite some time. Dave Inge <[log in to unmask]> Sent by: TechNet <[log in to unmask]> 08/25/2010 11:01 AM Please respond to Inge <[log in to unmask]> To [log in to unmask] cc Subject Re: [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT PARTS Dave, What's the idea with mixing Nickel and Palladium on component leads? In general, Pd is used as a substitute for Rhodium in order to increase the wear resistance for e.g. sliding contacts. I have also seen that mixing Ni an Pd causes an increase of the internal stress, rather much, depending on the wt%. What pays for the extra process in this case? /Inge -------------------------------------------------- From: "David D. Hillman" <[log in to unmask]> Sent: den 25 August 2010 00:21 To: <[log in to unmask]> Subject: Re: [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT PARTS > Hi! Yes, I made the assumption that Jon really meant Pd and not Pt as I > haven't run into a NiPtAu surface finish on components yet. > > Dave > > > > "Stadem, Richard D." <[log in to unmask]> > 08/24/2010 04:54 PM > > To > TechNet E-Mail Forum <[log in to unmask]>, "[log in to unmask]" > <[log in to unmask]>, "Roberts, Jon (SA-1)" > <[log in to unmask]> > cc > > Subject > RE: [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT PARTS > > > > > > > Well, jeez, Dave. You beat me to it again. Except I was busy trying to > find my references to soldering with platinum, not palladium. > > -----Original Message----- > From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman > Sent: Tuesday, August 24, 2010 4:13 PM > To: [log in to unmask] > Subject: Re: [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT > PARTS > > Hi Jon! There are a couple things to remember when dealing with NiPdAu > surface finishes: 1) Pd diffuses very slowly into a tin/lead solder alloy. > > You may need to add a few seconds to your soldering process cycle time; 2) > > Adding an additional 5-10C of temperature will assist in the Pd diffusion > into the tin/lead solder alloy. You may need to increase your soldering > temperature depending on which soldering process you are using; 3) Some > flux material are not compatible with Pd materials. You may want to try a > different flux to see if you get an improved reaction; 4) Run a > solderability test per IPC JSTD 002 to make sure you have an acceptable > NiPdAu surface finish. When Texas Instruments first introduced the NiPdAu > surface finish, we had to make slight time/temperature/flux adjustments on > > our typical soldering processes to obtain our expected soldering results. > Good Luck. > > Dave Hillman > Rockwell Collins > [log in to unmask] > > > > > "Roberts, Jon (SA-1)" <[log in to unmask]> > Sent by: TechNet <[log in to unmask]> > 08/24/2010 12:41 PM > Please respond to > TechNet E-Mail Forum <[log in to unmask]>; Please respond to > "Roberts, Jon (SA-1)" <[log in to unmask]> > > > To > [log in to unmask] > cc > > Subject > [TN] SOLDERABLIITY ON NICKEL PLATIUM GOLD LEAD FINISH SMT PARTS > > > > > > > Have any of you experience difficulty in producing an acceptable solder > joint with Nickel platinum gold SMT lead finishes? We can rework at > least twice to achieve an acceptable condition. Lead free part but we > use a solder with lead. Any help is appreciated. Jon > > > This communication is intended only for use by the addressee(s) named > herein and may contain business confidential and/or legally privileged > information. If you are not the intended recipient of this e-mail, you are > > hereby notified that any dissemination, distribution, disclosure or > copying of this e-mail and its contents is strictly prohibited. If you > have received this e-mail in error, kindly notify the sender by replying > to this message. In addition, please permanently delete the message and > any attachments without copying or disclosing the contents. Thank you for > your cooperation. > THIS DOCUMENT AND/OR SHIPMENT MAY CONTAIN COMMODITY ITEMS, SOFTWARE OR > TECHNICAL DATA THAT IS CONTROLLED BY U.S. EXPORT LAW, AND MAY NOT BE > EXPORTED OUTSIDE THE UNITED STATES OR TO NON U.S. PERSONS WITHOUT THE > APPROPRIATE EXPORT LICENSE FROM EITHER THE U.S. DEPARTMENT OF STATE OR > DEPARTMENT OF COMMERCE. > > > ______________________________________________________________________ > This email has been scanned by the MessageLabs Email Security System. > For more information please contact helpdesk at x2960 or [log in to unmask] > ______________________________________________________________________ > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 > > for additional information, or contact Keach Sasamori at [log in to unmask] or > > 847-615-7100 ext.2815 > ----------------------------------------------------- > > > > ______________________________________________________________________ > This email has been scanned by the MessageLabs Email Security System. > For more information please contact helpdesk at x2960 or [log in to unmask] > ______________________________________________________________________ > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 > for additional information, or contact Keach Sasamori at [log in to unmask] or > 847-615-7100 ext.2815 > ----------------------------------------------------- > > > > ______________________________________________________________________ > This email has been scanned by the MessageLabs Email Security System. > For more information please contact helpdesk at x2960 or [log in to unmask] > ______________________________________________________________________ > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 > for additional information, or contact Keach Sasamori at [log in to unmask] or > 847-615-7100 ext.2815 > ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------