Hi Eldon, I am surprised you ave not seen failures like these earlier. Also, did you perhaps switch to Pb-free solders? My present theory is the crack occurs when the assembly is wave soldered causing excessive tension on the resistor due to CTE mis-match, and some of these crack. Sorry, but this is wrong. On heating the PCB expands more than the CC—no cracking. But when the board comes back to ambient it seems to be longer, and shows a gap. On cooling, the PCB shrinks more, putting the CC, solder joints and all in tension—causes cracking and gaps. After a board goes through 3 heat cycles at a CM, wouldn't it be stable in CTE? No, there is no 'stabilization' of CTE's. And why would the other resistor not have the same issue? Is CTE different in X and Y? There are differences in CTE in x and y—by sometimes more than 2 ppm/C. The loading is also different if running parallel or perpendicular to the wave Finally, would an error or change in the raw fab process cause a change in the CTE and cause this issue to occur after many years? Obviously, something has changed—you need to find out what. Werner -----Original Message----- From: Eldon Sanders <[log in to unmask]> To: [log in to unmask] Sent: Fri, Jul 2, 2010 7:31 pm Subject: [TN] Cracked 2208 smt resistor end joint We are experiencing fractures in the end metallization or solder joint on one of two larger high voltage resistors, size 2208. They are mounted on FR-4. Only one location is failing. The other location is an inch away and oriented at 90 degrees. The failure rate is variable between assembly lots. Some have no failures, and no observed cracks. The most recent lot has a 2% failure rate, and another 2% that exhibit visible cracks in the ceramic but the solder joint is connecting the pad to the metallization and making electrical connection. I believe the root cause is the poor choice of the FR-4 board material with such a large ceramic resistor. However, about 80,000 boards have been built over 7 years without this failure mode. So, I am searching for the root cause of this specific timeframe. I have verified the process at the CM has not changed - the resistor is mounted on the 2nd pass SMT, and the board goes through wave soldering of TH components using a fixture. The same date code resistor is used for both good assembly lots and bad. There is some correlation to the date code of the bare fab. On cracked boards there is a gap observable between the solder joint and the ceramic resistor body. My present theory is the crack occurs when the assembly is wave soldered causing excessive tension on the resistor due to CTE mis-match, and some of these crack. But when the board comes back to ambient it seems to be longer, and shows a gap. After a board goes through 3 heat cycles at a CM, wouldn't it be stable in CTE? And why would the other resistor not have the same issue? Is CTE different in X and Y? Finally, would an error or change in the raw fab process cause a change in the CTE and cause this issue to occur after many years? Thanks to all the incredible minds if TechNet. Eldon Sanders Sr. Manufacturing Engineer Welch Allyn Monitoring 8500 SW Creekside Place Beaverton, OR 97008-7107 phone: (503) 530-7596 fax: (503) 526-4300 [log in to unmask] --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------