Those lids are made with holes in them, this is to stop the lid being forced off during a reflow cycle by the air under the lid expanding and breaking the bond line. The corrosion you are seeing is likely to be due to ingress of water during a water wash after reflow. The boards should be allowed to fully cool to room temp before entering the wash as if they are at a temperature above the wash water the cooling effect of the wash water will cool down the bga and the air under the BGA lid and could lead to water ingress as a result. Best regards, John Burke -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Roberts, Jon (SA-1) Sent: Wednesday, June 16, 2010 12:26 PM To: [log in to unmask] Subject: [TN] BGA AFTER 2 YEARS IN FIELD FAILED Has anyone experience a BGA failure after about 2 years, where under the heat sink of the actual part (metal lid) corrosion has occurred. The lid does pop off, if you applied some pressure to examine, and what we found was corrosion. There appears to be two weep holes on the inside of the part. Unless you have seen it you are probably going to ask me for some more information. I will try and obtain any pictures as long it as it does not show the manufacture. Thanks, Jon This communication is intended only for use by the addressee(s) named herein and may contain business confidential and/or legally privileged information. If you are not the intended recipient of this e-mail, you are hereby notified that any dissemination, distribution, disclosure or copying of this e-mail and its contents is strictly prohibited. If you have received this e-mail in error, kindly notify the sender by replying to this message. In addition, please permanently delete the message and any attachments without copying or disclosing the contents. Thank you for your cooperation. THIS DOCUMENT AND/OR SHIPMENT MAY CONTAIN COMMODITY ITEMS, SOFTWARE OR TECHNICAL DATA THAT IS CONTROLLED BY U.S. EXPORT LAW, AND MAY NOT BE EXPORTED OUTSIDE THE UNITED STATES OR TO NON U.S. PERSONS WITHOUT THE APPROPRIATE EXPORT LICENSE FROM EITHER THE U.S. DEPARTMENT OF STATE OR DEPARTMENT OF COMMERCE. ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------