Wayne, of course, you still need to divide by h [solder joint height] to get non-dimensional. The product does not give you any forces, just a displacement. How the combination of thin solder [with low modulus, but with ductility] and thin IMCs [with high modulus and low ductility] actually works is anybody's guess at this point in time. You can analyze it as purely a solder joint in creep-fatigue, as a brittle fully elastic high-strength loading of the IMCs, some combination thereof. But verification of whichever approach taken is critical. Werner -----Original Message----- From: Thayer, Wayne - IIW <[log in to unmask]> To: [log in to unmask] Sent: Fri, May 21, 2010 8:12 am Subject: Re: [TN] Solder joint height But if DCTE x DT is in units of delta L/L, and I multiply that by another L, then final units of your equation are in L. Something fails when stress (units of FORCE/(L x L)) exceeds a critical value. To get to this unit you usually use elastic modulus, which is units of (FORCE/(L x L))/(L/L). In a composite structure such as what we are talking about (part, board, solder), the overall elastic modulus is usually driven by the lowest elastic modulus in the system. For a BGA, it is obvious that elastic modulus is unimportant, because the net resisting force of the balls (due to both relatively low elastic modulus and relatively large height) is so much less than the forces developed by the DCTE stress that we can assume it is negligible: The balls will shear as dictated by your initial equation. But for the QFN and LCC condition, my intuition causes me to wonder if the elastic modulus of the solder is also important, particularly since you pointed out in the paper I referenced earlier that the intermetallics due to very thin solder joints are much stronger than the bulk solder. So should I interpret your response as the strength of the intermetallics is still not significant when analyzing QFN/LCC mountings? Wayne ________________________________ From: Werner Engelmaier [mailto:[log in to unmask]] Sent: Friday, May 21, 2010 7:35 AM To: [log in to unmask]; Thayer, Wayne - IIW Subject: Re: [TN] Solder joint height DNP stands for distance from neutral point. Werner -----Original Message----- From: Thayer, Wayne - IIW <[log in to unmask]> To: [log in to unmask] Sent: Fri, May 21, 2010 7:12 am Subject: Re: [TN] Solder joint height Thanks for your reply, Werner. DNP? I'm trying to figure that one out. Something to do with elastic modulii? Or is it number of cycles? I got the 1.5mil number from the Amkor paper, BOARD LEVEL ASSEMBLY AND RELIABILITY CONSIDERATIONS FOR QFN TYPE PACKAGES. Someone pointed that paper out on this forum a few months ago. That's why I decided to try the pin probe technique. Wayne ________________________________ From: Werner Engelmaier [mailto:[log in to unmask]<mailto:[log in to unmask]>] Sent: Thursday, May 20, 2010 6:30 PM To: [log in to unmask]<mailto:[log in to unmask]>; Thayer, Wayne - IIW Subject: Re: [TN] Solder joint height Hy Wayne, Well, those QFNs and LCCs are deja vu all over again. With LLCCCs we had an obvious huge CTE-mismatch between ceramic and FR-4, with QFNs it is not so obvious since the CTE-mismatch comes from the die--so die size and die attach are a big part of the equation. So it depends on the stresses developed by the thermal expansion mismatch from the product of DNPxDCTExDT whether the thin SJs will survive long enough for reliability. Werner -----Original Message----- From: Thayer, Wayne - IIW <[log in to unmask]<mailto:[log in to unmask]>> To: [log in to unmask]<mailto:[log in to unmask]> Sent: Thu, May 20, 2010 4:17 pm Subject: [TN] Solder joint height Should there be a spec for minimum solder joint height for leadless components? An old paper from Werner (mid 90's, I believe) popped up on the Internet when I queried this, and Werner has a statement in it that joints less than about 50 microns thick are basically all intermetallics, but that is not necessarily a bad thing since the intermetallics are stronger than the solder (but more brittle). I figured since we often try to get additional height for BGA joints to improve reliability, we should be concerned about QFNs and LCCs. I grabbed a 1.5mil (37 micron) tungsten rod out of our cleanroom (used for clearing clogged wirebond capillaries)and started seeing if I could get that under my leadless components. Couldn't get it under any of them, likewise with the QFNs. Checked Technet archives and didn't see an obvious thread, but maybe I didn't have the correct search parameters--if you just enter "height" you get a couple of thousand hits. Wayne Thayer This e-mail and any files transmitted with it may be proprietary and are intended solely for the use of the individual or entity to whom they are addressed. If you have received this e-mail in error please notify the sender. Please note that any views or opinions presented in this e-mail are solely those of the author and do not necessarily represent those of ITT Corporation. The recipient should check this e-mail and any attachments for the presence of viruses. ITT accepts no liability for any damage caused by any virus transmitted by this e-mail. ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask]<mailto:[log in to unmask]><mailto:[log in to unmask]<mailto:[log in to unmask]>> ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask]<mailto:[log in to unmask]><mailto:[log in to unmask]<mailto:[log in to unmask]>> with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]<mailto:[log in to unmask]><mailto:[log in to unmask]<mailto:[log in to unmask]>>: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]<mailto:[log in to unmask]><mailto:[log in to unmask]<mailto:[log in to unmask]>>: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask]<mailto:[log in to unmask]><mailto:[log in to unmask]<mailto:[log in to unmask]>> or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask]<mailto:[log in to unmask]> ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask]<mailto:[log in to unmask]> with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask]<mailto:[log in to unmask]> or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ______________________________________________________________________ This email has been scanned by the MessageLabs Email Security System. For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------