Hi Guy! Yes the ROSA (Reduced Oxide Soldering Activation) process would be able to restore a HASL surface finish but I probably have the only remaining functioning system in the industry. Secondly, you need to process the "restored" pwb within a few hours after ROSA treatment or the effectiveness is lost . I could restore Lee's pwb solderability but I couldn't get it shipped to him in time before it would it would re-oxidized. As several other TechNet contributors have suggested, a very controlled re-HASL process with the correct flux and cleaning processes could be a potential option. Dave Guy Ramsey <[log in to unmask]> Sent by: TechNet <[log in to unmask]> 12/10/2009 06:55 PM Please respond to TechNet E-Mail Forum <[log in to unmask]>; Please respond to Guy Ramsey <[log in to unmask]> To [log in to unmask] cc Subject Re: [TN] BOARD SOLDERABILITY Remember that tank we had at ACI that was did electrochemical reduction. It was a Rockwell invention I think, ROSA? It could restore solderability to some metals. I don't know how it would get through the HASL. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Lee Whiteman Sent: Thursday, December 10, 2009 1:54 PM To: [log in to unmask] Subject: [TN] BOARD SOLDERABILITY One of my colleagues has a HASL finished board, that sat in our stockroom for ~ 10 years, and of course he want to use them (EOY Billing). Ran the board through wave soldering, and it did not solder at all. Good news was that the board was not damaged by the heat - it just was not solderable. I do not want to use a more active flux since it will be difficult to clean. Are there any solutions / processes that can restore board solderability? Thanks in advance. Lee Whiteman, PMP Senior Member Engineering Staff L-3 Communications East Telephone: (856) 338-3508 FAX: (856) 338-2906 E-Mail: [log in to unmask] --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------