Chris, In that particular case the surface roughness does matter a lot. Ideally, an indenter should come at 90 degree to the surface and it wouldn't be the case particularly for ENIG with its "nodding structure". In addition, as I said before you can not compare the numbers as (in case of ENIG) the reading most probably will be affected by residual stresses. I'm not aware of a "typical" number for ENIG. A number of years ago I tried to measure it at different loads but don't remember what the readings were. Honestly, I wouldn't use nanohardness (great technique but for different tasks) in your particular case. Regards, Vladimir SENTEC SENTEC 11 Canadian Road, Unit 7. Scarborough, ON M1R 5G1 Tel: (416) 899-1882 Fax: (905) 882-8812 www.sentec.ca -----Original Message----- From: Chris Mahanna <[log in to unmask]> Date: Mon, 2 Nov 2009 22:12:04 To: <[log in to unmask]> Subject: Re: [TN] IAu hardness Vladimir, Indeed nano. Both platings were tested with the exact same protocol: Berkovich geometry, 1mN max load. They are reporting penetration depth in nM. The lab complained about the surface being too rough. Might the IAu be un-uniform and the indenter is getting ahold of some Ni? XRF with 4mil collimator doesn't show anything odd. Saw some mudcracks via SEM on a "related" sample. Or, should we just punt and say that comparisons can't be made? If so, does anyone know what numbers you typically get from ENIG? Chris -----Original Message----- From: [log in to unmask] [mailto:[log in to unmask]] Sent: Monday, November 02, 2009 9:34 PM To: TechNet E-Mail Forum; Chris Mahanna Subject: Re: [TN] IAu hardness Hi Chris, Are you sure you are talking about nanohardness and not microhardness? If it's nanohardness, then the measured values are completely different from a common (microhardness) method due to the nature of nanohardness measurements. Secondly (and even more important) on a plated sample (and particularly like ENIG with extremely thin layer of Au) the nanohardness readings will depend on the indentation load (read depth of penetration). In general, you can not draw a direct comparison between nanohardness measurements done on a thick (your hard gold case) and extremely thin (ENIG case) plating. Regards, Vladimir ------Original Message------ From: Chris Mahanna Sender: TechNet To: [log in to unmask] ReplyTo: TechNet E-Mail Forum ReplyTo: Chris Mahanna Sent: Nov 2, 2009 21:17 Subject: [TN] IAu hardness Please help a simple EE. From bare printed boards we are receiving nano-identation (hardness) values for hard (I assume Cobalt) gold in the 3000 MPa range. Quick and dirty conversion yields ~300 Knoop/Vickers; right? That sounds reasonable. BUT, we're getting 6500 MPA for the ENIG. Is this even possible? Does anyone know if it is an indication of poor IAu? Or maybe a poor nano-indentation tester? Thanks, Chris --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- SENTEC 11 Canadian Road, Unit 7. Scarborough, ON M1R 5G1 Tel: (416) 899-1882 Fax: (905) 882-8812 www.sentec.ca --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------