Hi Inge! Sorry for the these tardy comments (I took advantage of the Labor Day holiday here in the US and enjoyed a 4 day weekend of whitewater kayaking in Wisconsin) but hopefully they add to the information already provided: 1) Immersion Tin PWB Surface Finish - ImSn is a viable pwb surface finish and is used on a wide variety of IPC Class 1/2/3 products. However, ImSn does not have the greatest thermal excursion robustness and long term solderability shelf life - both issues due to the oxidation of the Sn and/or the oxidation of SnCu intermetallic phase (copper and tin diffusion interactions). There are a multitude of ImSn plating chemistries on the market and they are not all "equal" in terms of oxidation and tin whisker resistance. I highly recommend that before using an ImSn surface finish the oxidation and tin whisker issues be completely investigated. Correctly formulated and processed ImSn chemistries should not have tin whiskers and should have a 12 month solderability shelf life. 2) Pressfit Pin and PWB Surface Finishes - all of the pwb surface finishes - OSP, ImSn, ImAg and ENIG can be used with pressfit pin technology. As Bev described, very close attention must be paid to the plated thru hole dimensions/tolerances to insure that a successful pressfit pin process can be achieved. And yes, if no attention to the hole dimensions/tolerances is conducted, you get damaged holes and damage laminate. Rockwell Collins uses pressfit pins with the ImSn, ImAg and ENIG surface finishes successfully on a number of product designs. Dave Hillman Rockwell Collins [log in to unmask] Hernefjord Ingemar <[log in to unmask]> Sent by: TechNet <[log in to unmask]> 09/07/2009 06:21 AM Please respond to TechNet E-Mail Forum <[log in to unmask]>; Please respond to Hernefjord Ingemar <[log in to unmask]> To [log in to unmask] cc Subject [TN] Need clever comments Hi all, need some professional backup regarding MIL quality boards. Objects: FR-4 Class III double-sided multi-layer boards, populated with SOICS, BGAs,and a lot of passive components. Observation 1 : the non soldered board have lots of Tin whiskers on inside of the PTH barrel. My thought is this: if whiskers can grow long before the board is assembled, then ain't it likely that even CAF can be generated? See photo 1. Observation 2: Copper has somehow penetrated the solder mask. This can be found everywhere along the conductor traces. You need a very good light microscope and a SEM to see it. See photo 2. Board data: Copper with 0.8 micrometer Immersion Tin. No nickel barrier. Solder mask thickness not specified. Application: Typical MIL-883 environment Q1: What is your opinion about that thin Tin directly on copper? I dislike the concept. Copper is very mobile at high temperatures, and combined with humidity, there can be leakage currents and corrosion issues. Even if the boards are CCd, there is a risk with copper . Q2: I gave the advice to introduce a nickel barrier, but our customer claimed, that they can't because of pressfit connectors and pressfit test pins on the board. Furthermore, they had heard that one cannot have nickel platings when pressfitting, because the nickel will crack and oxidize and cause electrical disfunction. Is this your opinion too? Are there any relevant testing behind such statements? Thanks in advance Inge --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------