Lieber Herr Jeremias, Ich stimme Ihnen zu. Weil vielleicht die Goldversprödung keinen Funktionsausfall bei Durchlöchern herbeiführt, kann es doch zu einem Totalbruch führen. Ich würde dem Zulieferer vorschreiben auch bei kleineren Goldschichtdicken als 2,5 µm zu entgolden. Hinsichtlich der Normen, wenn man etwas darin finden will, muss man sich daran beteiligen um es durchzudrücken. Regards, Werner Engelmaier Engelmaier Associates, L.C. Electronic Packaging, Interconnection and Reliability Consulting 7 Jasmine Run Ormond Beach, FL 32174 USA Phone: 386-437-8747, Cell: 386-316-5904 E-mail: [log in to unmask], Website: www.engelmaier.com -----Original Message----- From: Jeremias, Michael <[log in to unmask]> To: [log in to unmask] Cc: [log in to unmask] Sent: Tue, Aug 4, 2009 12:14 pm Subject: WG: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT Lieber Herr Engelmaier, In der J-STD-001 steht: 3.9.3 Gold Removal Gold shall13 be removed: • From at least 95% of the surface to be soldered of the through-hole component leads with 2.5 μm [0.0984 mil] or more of gold. • From 95% of all surfaces of surface mount components to be soldered regardless of gold thickness. • From the surface of solder terminals plated with 2.5 μm [0.0984 mil] or more of gold. A double tinning process or dynamic solder wave may be used f or gold removal. Electroless nickel immersion gold (ENIG) finishes on PCBs are exempt from this requirement. These requirements may be eliminated if there is documented objective evidence available for review that there are no gold related solder embrittlement problems associated with the soldering process being used. (13) Class 1-Not Est Class 2-Proc Ind Class 3-Defect Das heisst ein Zulieferer, der nach J-STD-001 liefert darf auf den Entgoldungsprozess verzichten, wenn bei through hole componenten die Goldschichtstärke unter 2,5 µm z, B 2,4 µm beträgt. Ist das wirklich so zulässig? Oder sollen wir unserem Zulieferer vorschreiben auch bei kleineren Goldschichtdicken als 2,5 µm zu entgolden. Sie schreiben doch, dass selbst bei bei viel kleineren Durchschnittsgrössen als 3wt% Goldversprödung vorkommen kann. Und mit 2,5 µm Goldschichtstärke lässt sich das in einem engen PTH nicht erreichen, da die Lofüllung nicht ausreicht. Sie schreiben auch, dass die Gefahr besteht, dass das Gold nicht gleichmässig verteilt sein kann. Das wirkt sich natürlich bei Feinpitch BAuelemneten umso mehr aus. Dann sollte das auch in den Normen so stehen. Sincerly Michael Jeremias Industrial Engineering (OPPI41) Electronics Production ((( Defence Electronics EADS Deutsc hland GmbH 89077 Ulm Tel.: +49 (0) 7 31.3 92-5533 Fax: +49 (0) 7 31.3 92-73 15 E-Fax: +49 (0) 7 31.3 92-20 5533 -----Ursprüngliche Nachricht----- Von: TechNet [mailto:[log in to unmask]] Im Auftrag von Werner Engelmaier /* Gesendet: Dienstag, 4. August 2009 13:44 An: [log in to unmask] Betreff: Re: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT Lieber Herr Jeremias, 1. Es ist nicht leicht ein IEC Dukument zu ändern. 2. Die meistens Länder haben eine Vertretung bei der IEC die für solche Anfragen zuständig sind. Wie ich schon früher gesagt habe, sind diese Goldgrenzen von 1,6 vol% oder 3 wt% sehr grobe Daumenanpeilungen, und Goldversprödung kann bei viel kleineren Durchschnittsgrössen vorkommen, da in den meisten Fällen das Gold nicht gleichmässig verteilt ist. Ausserdem, ist diese Goldversprödung nicht eine Ja/NeinSache sondern brigt eine absteigende Gefügeschwächung. Regards, Werner Engelmaier Engelmaier Associates, L.C. Electronic Packaging, Interconnection and Reliability Consulting 7 Jasmine Run Ormond Beach, FL 32174 USA Phone: 386-437-8747, Cell: 386-316-5904 E-mail: [log in to unmask], Website: www.engelmaier.com -----Original Message----- From: Jeremias, Michael <[log in to unmask]> To: [log in to unmask] Sent: Tue, Aug 4, 2009 4:09 am Subject: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT Unfortunately, the discussion about the matter is not so serious as the problem. Proceedings in technological quality are not available by (hundreds!) of mails with ridiculous content but by hard work. 1, Who knows the responsible at IEC or TC91, who is able to change it? 2. Who is able to make thebchange request? Sincerly Michael Jeremias Industrial Engineering (OPPI41) Electronics Production ((( Defence Electronics EADS D eutschland GmbH 89077 Ulm Tel.: +49 (0) 7 31.3 92-5533 Fax: +49 (0) 7 31.3 92-73 15 E-Fax: +49 (0) 7 31.3 92-20 5533 P Before printing, think about the environment ! mailto: [log in to unmask] EADS Deutschland GmbH Registered Office: Ottobrunn District Court of Munich HRB 107 648 Chairman of the Supervisory Board: Dr. Thomas Enders Managing Directors: Dr. Stefan Zoller (chairman), Michael Hecht This E-mail and any attachment(s) to it are for the addressee's use only. It is strictly confidential and may contain legally privileged information. No confidentiality or privilege is waived or lost by any mistransmission. If you are not the intended addressee, then please delete it from your system and notify the sender immediateley. You are hereby notified that any use,=2 0 disclosure, copying or any action taken in reliance on it is strictly prohibited and may be unlawful. - Thank you. -----Ursprüngliche Nachricht----- Von: TechNet [mailto:[log in to unmask]] Im Auftrag von Joyce Koo Gesendet: Freitag, 31. Juli 2009 19:06 An: [log in to unmask] Betreff: Re: [TN] AW: [TN] AW: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT Who ever made doc and approved it should get shot at... seriously. Not a Friday joke. -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Jeremias, Michael Sent: Friday, July 31, 2009 12:17 PM To: [log in to unmask] Subject: [TN] AW: [TN] AW: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT Unfortunately it is not (!)=2 0a typo from me . The document DIN EN 61191-1 contains this value 2,5 µm . But I am not confident, that this is low enough for any process cases so we use for PTH the same rule as above as mentioned below Sincerely Michael Jeremias -----Ursprüngliche Nachricht----- Von: TechNet [mailto:[log in to unmask]] Im Auftrag von Joyce Koo Gesendet: Donnerstag, 30. Juli 2009 12:22 An: [log in to unmask] Betreff: Re: [TN] AW: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT Must be a typo. Should be 0.25 micron? 10 micro-inches? --------------- ----------- Sent using BlackBerry ----- Original Message ----- From: TechNet <[log in to unmask]> To: [log in to unmask] <[log in to unmask]> Sent: Thu Jul 30 04:26:14 2009 Subject: [TN] AW: [TN] FORMULA FOR DETERMINING GOLD PERCENTAGE IN A SOLDER JOINT IEC 61191-1 chapter 6.2.2 contains the rules < 1,4% Volume Au, < 3% Wt Au in the final solder interconnection < 2,5 µm for PTH Wave soldering (I am not confident, that this is low enough for any process cases so we use for PTH the same rule as above) You have to take into consideration solder paste volume(stencil-thickness), wetted Au-surface, wetted Au thickness Own investigations show, that Au brittelness may occure from 1,6% Vol and really will occure from 2,3% Vol. Sincerly Michael Jeremias Industrial Engineering (OPPI41) Electronics Production ((( Defence Electronics EADS Deutschland GmbH 89077 Ulm Tel.: +49 (0) 7 31.3 92-5 533 Fax: +49 (0) 7 31.3 92-73 15 E-Fax: +49 (0) 7 31.3 92-20 5533 P Before printing, think about the environment ! mailto: [log in to unmask] EADS Deutschland GmbH Registered Office: Ottobrunn District Court of Munich HRB 107 648 Chairman of the Supervisory Board: Dr. Thomas Enders Managing Directors: Dr. Stefan Zoller (chairman), Michael Hecht This E-m ail and any attachment(s) to it are for the addressee's use only. It is strictly confidential and may contain legally privileged information. No confidentiality or privilege is waived or lost by any mistransmission. If you are not the intended addressee, then please delete it from your system and notify the sender immediateley. You are hereby notified that any use, disclosure, copying or any action taken in reliance on it is strictly prohibited and may be unlawful. - Thank you. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847- 615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------------------------- This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-clie nt or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) d elivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------------------------- This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet s end e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet s end e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------