Looks like the mask is very thin over the traces. Hope you don't get failures there. Some of the circles look like the inner layer clearances, others look like contaminants. I think you need a X-section. Chuck Brummer 3M Manufacturing Engineer 8357 Canoga Ave. Canoga Park, CA 91304-2605 (818) 734-4930 Paul Reid <[log in to unmask]> Sent by: TechNet <[log in to unmask]> 06/19/2009 02:12 PM Please respond to TechNet E-Mail Forum <[log in to unmask]>; Please respond to Paul Reid <[log in to unmask]> To [log in to unmask] cc Subject Re: [TN] PCB problems Hi Ioan, I think the Halo looks like a contaminant and could be a problem. It might be thick mask but my vote says contaminant under the mask. Why not probe the mask and see if the discolorations is on the surface of the PWB or not. Best regards, Paul -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea Sent: Friday, June 19, 2009 3:49 PM To: [log in to unmask] Subject: [TN] PCB problems Dear Technos, I have a few questions regarding a funny lot of PCBs we've received. Steve was kind enough to post the pictures, see http://stevezeva.homestead.com/files/non_uniform_hasl.jpg < http://stevezeva.homestead.com/files/non_uniform_hasl.jpg> http://stevezeva.homestead.com/files/non_uniform_hasl_1.jpg < http://stevezeva.homestead.com/files/non_uniform_hasl_1.jpg> http://stevezeva.homestead.com/files/via_halo.jpg < http://stevezeva.homestead.com/files/via_halo.jpg> http://stevezeva.homestead.com/files/via_halo_detail.jpg < http://stevezeva.homestead.com/files/via_halo_detail.jpg> Out of the pack of 15 that I have inspected, most of them have some weird halos around all the vias, but no such issue around the component mounting holes. The pictures show the worst board, the rest have it to a lesser extent. What is it? Should this be a reject? Is this anything we should admonish our fab about? Secondly, the SnPb HASL, is irregular on the pads, which is not out of the ordinary, but on some boards looks like in the pictures. I hesitate calling this de-wetting, since the wetting angles are good. Is it de-wetting? Should we reject the boards? I will paste the worst board I find and reflow it, to get an idea what happens during soldering, but I should also be able to help the incoming inspectors draw a line between good and bad in visual inspection of future lots... Thank you, Ioan Tempea, ing. Ingénieur Principal Fabrication / Sr. Manufacturing Engineer 30 ans déjà! - Already 30 years! 950 rue Bergar, Laval, Québec, H7L 5A1 t : 450-967-7100 ext : 244 Mtl : 514-990-5762 f : 450-967-7444 [log in to unmask] <mailto:[log in to unmask]> www.digico.cc <http://www.digico.cc/> P N'imprimer que si nécessaire - Print only if you must --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------