Genny, We have experienced a very similar phenomenon on one of our product boards. The BGA was 1.3" square, and there was pad cratering along the corner pads. The laminate was a high Tg, with added filler to minimize Z-axis CTE. Chaning the laminate was not an option, so we had to come up with a process solution to the problem. We determined that the cratering was not occurring during reflow cool down (but was later, at a indeterminate process step during board assembly). We did a simple set of expts with 3 random replications of each: 1. corner bonding prior to reflow (chipbonder 3609) 2. corner bonding immediately after reflow 3. using a SMT pallet throuout the process (so as to eliminate handling stresses) We made sure that at least 1/4th length of each BGA side was covered by the bonding material. In all 3 cases we could manufacture 100% defect free product. Then based on the simplicity, corner bonding after reflow was instituted as the preferred stress mitigation technique. Might be worth a shot to do something similar. Regards, Amol -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Genny Gibbard Sent: Thursday, June 11, 2009 4:10 PM To: [log in to unmask] Subject: [TN] Corner ball pad cratering Hello all, If you have identified a BGA with corner ball pad cratering, what would be your suggestions to correct this condition? Our thoughts: 1. We plan to evaluate our handling processes to reduce/remove excessive flex/strain occurring around this part 2. We plan to evaluate corner bonding or underfilling for the BGA. Which do you feel would be the best direction to go? Do you have other suggestions? Thanks in advance for all your help Genny --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- WARNING: Export Control This document may contain technical data within the definition of the International Traffic in Arms Regulations (ITAR), and subject to the Export Control Laws of the U.S. Government. Transfer of such data by any means to a foreign person, whether in the United States or abroad, without proper export authorization or other approval from the U.S. Department of State is prohibited. CONFIDENTIALITY NOTICE: This e-mail, and any attachments, is for the sole use of the intended recipient(s) and may contain information that is confidential and protected from disclosure under the law. Any unauthorized review, use, disclosure, or distribution is prohibited. If you are not the intended recipient, please contact the sender by reply e-mail, and delete/destroy all copies of the original message and attachments. Thank you. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------