To understand this problem, you also need to understand what happens when synthetic polymers are heated. What I am about to say applies equally to solder masks and to the substrates under them. When a polymer is heated, it reaches a temperature where its characteristics change, called the glass transition temperature. Above this temperature, the surface of a polymer becomes very porous and opens up like a sponge. To make things worse many of the chemicals that the polymer comes in contact with contain surfactants or other molecules which have a hydrophilic and lipophilic ends. If the molecule is linear, or nearly so, such as most of the common detergents and surfactants, another phenomenon occurs and the lipophilic end of hundreds of molecules rush into the pores and are trapped there when the polymer cools again. If, for example, the product is a flux, then some activators will probably become co-trapped and these can be released, not only with subsequent heating, but also at ambient temperatures over a long period of time. This is obviously a danger for the reliability of any printed circuit in critical applications. In addition, just to make things worse, many thermosetting polymers have ionic salts in their molecular makeup. For electrical applications, these salts are practically eliminated but there is always a risk of small quantities remaining and these can also leach out. Other posts have specifically mentioned HASL. This is because the fluxes used for this process are not only highly activated but nearly all the other chemicals in them are closely related to surfactants! You've got the worst of both worlds! What can be done about them? Not a great deal if you have a batch of circuits that leach enough to compromise the functionality. Perhaps a good wash in DI water after having baked the circuits may improve the situation if the problem comes from the fabricator. If it comes from your own workshop, then a systematic tracing will find the culprit. Hope this helps! Brian Kane, Joseph E (US SSA) wrote: > A cleaned bare PB is exposed to bake or reflow, and comes out with > measurable ionic contamination. The board is dirtier at the surface > after > a heat excursion. > > The contamination isn't coming from the oven, handling, or anything > external. > Heat causes something to move from the inside of the board to the > outside. > > We haven't done any ion chromatography or other testing yet to > run this down, but has anyone heard of or experienced anything similar? > > In our normal process, we clean everything multiple times, but if the > contaminant builds up under solder mask, or in other areas that are > difficult to clean, we could have SIR or corrosion problems around fine > surface features or in high voltage areas. > > And if this ionic contamination doesn't just move up to the surface, > but is somehow moving around inside the board, could it collect in > some places and lead to CAF or other problems? > > Joe Kane > BAE Systems > Johnson City, NY > > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 > ----------------------------------------------------- > --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------