Hi Inge, I'm curious how you are going to prove that your part is "clean" once all your cleaning is done. If the oils are tenacious and imbedded in the surface of the titanium how do you plan to test for them? KennyB -----Original Message----- From: Brian Ellis [mailto:[log in to unmask]] Sent: Monday, March 30, 2009 7:40 AM To: [log in to unmask] Subject: Re: [TN] Titanium Titanium is a funny metal. Fabricated items, such as snob-value watch cases, are often sintered into a rough shape before machining, rather than cast, as would be gold. This is because casting is very expensive as it is done in a vacuum (hot Ti burns on O2 and N2 long before its melting point!!!). Ti is extremely difficult to machine, whether sintered or derived from a casting, but sintered is the worst. The tool must be really perfectly ground without wear and the Ti must be really well cooled (pumped cutting oil systems such as for steel or non-ferrous metals are often insufficient). This is because there is a phase change induced by pressure at temps above ambient, locally softening the metal crystal-by-crystal and this causes the metal to deform onto the tool and gall. This often 'snowballs' by minor galling inducing ever-increasing deformation. I don't know all the ins and outs of Ti galling but I have observed it as a severe problem in practice (in a former life, I designed a part for working in HCl that had to be turned from bar; the turner had hell's own job!). I mention this because your "squamous" surface may be due to galling, especially if the part is sintered, rather than cast. As for TCE, I knew one of the guys who was behind the ban in Sweden. At the time, I had long and heated discussions with him that he was making a BIG mistake. I never was a fan of halogenated solvents but I always admitted there were some applications for which they were indispensable. The idiocy started in E Germany where a factory's employees had an abnormal number of cancer cases ascribed to TCE. No epidemiological study was made or confounding factors determined. It later transpired that the TCE was stabilised with epichlorohydrin, a known carcinogen but it was too late, Germany had already decreed TCE was a known carcinogen in humans (MAK1) with a PEL of (I think) 1 ppm. For some reason, they never wanted to correct this error, despite serious studies to the contrary, and some other countries followed suit. FYI, perc, which is potentially more toxic than TCE, is classed as MAK3 in Germany with a PEL of 25 ppm. Carbon tetrachloride, which is KNOWN to be a lot more toxic than TCE, is also classed as MAK3 with a PEL of 10 ppm. It simply makes no sense whatsoever. I think you will find Germany's stupid classification of TCE will reach REACH, if it hasn't already done so. To get back to my Swedish colleague, he argued that all applications using TCE could be replaced by aqueous cleaning methods. Memories of these arguments still make me squirm; you simply could not have a scientific discussion based on fact, he had a political point to make. At one point, in a committee meeting with ~20 persons present, he was shot down in flames by the consensus and he simply stormed out of the room, slamming the door (this was c. 1989, when we were desperately trying to promote all known means of cleaning using relatively safe non-ozone depleting solvents, such as TCE, in preference to 1,1,1-TCA). Would it be possible to use TCE in a zero-emissions machine? (Virtually 0 ppm in the workshop at all times, certainly less than 1 ppm.) Surely that cannot be forbidden? It would also ensure compliance with the EU VOC Directive. Brian Hernefjord Ingemar wrote: > I reckon that some mineral oils seem to be very bullheaded. We had let parts pass aceton and etanol and some other cleanings, and to our surprise, after electron beam vacuum welding the two (cleaned)parts together, small and yellowish fatty things appeared on the liquid surface when the finished part was recleaned after the welding. This was done by dipping the flasklike part in a degreasing tank. Evidently, mineral oil was still hidden in the titanium surface after machining, despite it looked clean and left no debris when you rubbed with a white cloth. In a high magnification microscope you can see a lot of microscopic damages, void or what to call the rude surface. Just unlike steel and other metals. Whatever machining parameters or tools, it seeems as titanium is "squamous" after the drilling, milling etc. > > TRI...hmm...was cast out here twenty years ago...chemo textile cleaning is allowed to be done with perchloroethylene, which I find remarkable. The later is not better in a environmental point of view. > > Inge > > PS. VIGON 200 = 11-12 (pH) > > -----Original Message----- > From: TechNet [mailto:[log in to unmask]] On Behalf Of Brian Ellis > Sent: måndag 30 mars 2009 13:04 > To: [log in to unmask] > Subject: Re: [TN] Titanium > > I'm not sure that Vigon will be satisfactory for removing mineral oil residues and their additives, as these will not saponify in the amines. > You will need something with the pH exceeding 12-13 and with stronger tensio-active components. > > I'll shock you by suggesting a trichloroethylene blend in a zero-emissions cleaning machine with a vapour phase final. I don't care what people say, it is a damned good low-cost solvent, used sensibly it is perfectly safe, it is non-carcinogenic to humans (it is carcinogenic to rodents in high doses, but their metabolism of the substance is > different) AND IT WORKS!!! (If needed, I have details of epidemiological studies with cohorts of tens of thousands supporting my statements.) > > In the unlikely event that this alone would be insufficient for your needs, then consider an aqueous solution, depending on the residue analysis after TCE. > > Brian > > This alone would probably be sufficient and low-cost > > Hernefjord Ingemar wrote: >> The tests will show. If one or two steps can be left, of course very good. On the other hand, the cost for these units is so high, that some dollars saving is negligible. Unlike the normal production when cents are hunted for. >> >> The alcaline bath will possibly be superseded by our Vigon 200 tunnel cleaner. >> /Inge >> >> -----Original Message----- >> From: TechNet [mailto:[log in to unmask]] On Behalf Of R Sedlak >> Sent: måndag 30 mars 2009 11:28 >> To: [log in to unmask] >> Subject: Re: [TN] Titanium >> >> Ingmar: >> The process you suggest probably will work, but I suspect it is overkill. I suspect that the alkaline cleaner will be enough on its own. >> >> Good luck. >> Rudy Sedlak >> >> --- On Sun, 3/29/09, Hernefjord Ingemar <[log in to unmask]> wrote: >> >> From: Hernefjord Ingemar <[log in to unmask]> >> Subject: Re: [TN] Titanium >> To: [log in to unmask] >> Date: Sunday, March 29, 2009, 11:58 PM >> >> Thank you, Rudy&Steve. >> >> It seems as a suitable treatment would be this one: >> a)Solvent degrease, followed by >> b)Alcaline bath, followed by >> c)DI ultrasonic bath, followed by >> d)Micropowder blast, followed by >> e)HNO3 dip, followed by >> f)DI ultrasonic bath. >> >> We will try this today already. We do not like HF, so that kind of process is skipped. Our problem is not primarily to remove the oxide, but to ascertain that all threading/cutting oil is gone, also that the numerous micro pores are emptied from their content. >> >> /Inge >> >> >> >> >> -----Original Message----- >> From: TechNet [mailto:[log in to unmask]] On Behalf Of R Sedlak >> Sent: lördag 28 mars 2009 20:19 >> To: [log in to unmask] >> Subject: Re: [TN] Titanium >> >> Although Titanium lightly alloyed is used in some joint replacements, it may well be more commonly known for its use as Nitinol, a Nickel/Titanium alloy, which has weird "memory" properties. Nitinol is one of the more common stent materials. >> >> Cleaning Titanium is quite difficult, particularly if it is heavily oxidized, as the common "cleaning" agent, (Hydrofluoric Acid) attacks Titanium vigorously, and then to frost the cake, this causes Hydrogen embrittlement. >> >> Not everyone/everywhere is as "enlightened" as we like to think we are, and yes, there is still choro-ethanes still in use in cleaning (Think "dry cleaning" clothes). >> >> There are proprietary cleaners which purport to get around these issues. If interested, contact me off Technet. >> >> Rudy Sedlak >> RD Chemical Company >> >> >> >> >> >> >> >> --------------------------------------------------- >> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To >> unsubscribe, send a message to [log in to unmask] with following text in >> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt >> or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET >> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the >> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the >> archives of previous posts at: http://listserv.ipc.org/archives Please >> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 >> for additional information, or contact Keach Sasamori at >> [log in to unmask] or 847-615-7100 ext.2815 >> ----------------------------------------------------- >> >> --------------------------------------------------- >> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To >> unsubscribe, send a message to [log in to unmask] with following text in >> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt >> or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET >> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the >> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the >> archives of previous posts at: http://listserv.ipc.org/archives Please >> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 >> for additional information, or contact Keach Sasamori at >> [log in to unmask] or 847-615-7100 ext.2815 >> ----------------------------------------------------- >> >> >> >> >> >> --------------------------------------------------- >> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To >> unsubscribe, send a message to [log in to unmask] with following text in >> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt >> or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET >> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the >> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the >> archives of previous posts at: http://listserv.ipc.org/archives Please >> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 >> for additional information, or contact Keach Sasamori at >> [log in to unmask] or 847-615-7100 ext.2815 >> ----------------------------------------------------- >> >> --------------------------------------------------- >> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To >> unsubscribe, send a message to [log in to unmask] with following text in >> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt >> or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET >> Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the >> posts: send e-mail to [log in to unmask]: SET Technet Digest Search the >> archives of previous posts at: http://listserv.ipc.org/archives Please >> visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 >> for additional information, or contact Keach Sasamori at >> [log in to unmask] or 847-615-7100 ext.2815 >> ----------------------------------------------------- >> > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 > ----------------------------------------------------- > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 > ----------------------------------------------------- > --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------