Kevin, Dyne pens are generally bought as a set and they look much like magic markers or highlighter pens. Each contains a different solution with different surface tensions. You start with a 30 pen and draw a strip of the fluid on the surface. If the solution has not beaded up, then you go to the 32 pen, and continue until you find the solution where beading occurs. The sets that I use go from 30 dynes/cm to 44 dynes/cm. If pen 38 did not bead and pen 40 does, the surface tension was 39 dynes/cm. It is a quick way to check a surface and the inks are easily cleaned off. I have found that for many surfaces, you get pretty good adhesion (depending on the coating) for surface tensions of 40 or better. Tensions of 35-40 are marginal. Tensions of 30-35 are more problematic. Tensions below 30 are "good luck Charlie". A decent set of pens runs about $150. The water break test you describe is a quick and inexpensive qualitative check on a surface, but not quantitative. When I do more quantitative evaluations of surface cleanliness, I would prefer to use a device called a goniometer, which measures the contact angle of a drop of DI water on a surface. A clean surface has a very low contact angle, a dirty or difficult surface has a high contact angle. This is different from a goony-ometer, which largely checks to see if Dewey is anywhere around. Though, admittedly we have a hell of a time calibrating it if either Hillman or I are within a mile of the darn thing. Doug Pauls Rockwell Collins Kevin Glidden <[log in to unmask]> Sent by: TechNet <[log in to unmask]> 02/06/2009 08:01 AM Please respond to TechNet E-Mail Forum <[log in to unmask]>; Please respond to Kevin Glidden <[log in to unmask]> To [log in to unmask] cc Subject Re: [TN] Coating material Doug - I am not familiar with dyne pens...can you explain? I have also heard of a simpler test called the water break test. Literally all you do is get a sample of DI water and pipette a few drops onto the PCB surface. You are looking for the water to spread and wet to the PCB surface, indicating it is free of contaminants. If it beads up (like on a well waxed car), then it is indication of a film or contaminant that would result in poor coating. I am not certain how different solder mask materials effect the results of this test, but you can't argue the cost and simplicity. Kevin Glidden Manufacturing Engineer Luminescent Systems Inc. -----Original Message----- From: Douglas Pauls [mailto:[log in to unmask]] Sent: Thursday, February 05, 2009 5:33 PM To: [log in to unmask] Subject: Re: [TN] Coating material Ted, Where do you see the dewetting and what processes come before coating? In my experience, dewetting comes three general sources: 1. A problem with the surface energy of the component or solder mask. This may be due to mold release agents or the slick nature of the plastic itself. You want surface energies in excess of 40 dynes/cm. Surface energies of 30-35 dynes/cm are a problem. I use Dyne Pens as a quick check. Has there been a change in process or part supplier? 2. A problem with a barrier material. Again, it may be a mold release agent, many of which are Teflon or sulfur based, or it may be a process residue. Could be silicone residues, could be fingerprints, could be any number of things from second or third shift. 3. Dewey Whittaker. Doug Pauls Rockwell Collins Ted Tontis <[log in to unmask]> Sent by: TechNet <[log in to unmask]> 02/05/2009 03:56 PM Please respond to TechNet E-Mail Forum <[log in to unmask]>; Please respond to Ted Tontis <[log in to unmask]> To [log in to unmask] cc Subject Re: [TN] Coating material We are experiencing de-wetting upon application. We are using a PVA coater and using the same ratio, 1 to 1. The problem is that it is interment within the same lot making it difficult to pin down. Samples of bare boards as well as boards that coated fine and ones that coated poorly have been sent out to a lab for eval. Ted -----Original Message----- From: Tom P. Hummel [mailto:[log in to unmask]] Sent: Thursday, February 05, 2009 2:45 PM To: TechNet E-Mail Forum; Ted Tontis Subject: RE: [TN] Coating material We currently use HumiSeal 1B73AP thinned 1 to 1 with 521 in our PVA machine and have not had any issues. Are you experiencing problems? What type of automated machine are you using? Thomas P. Hummel Carlton Industries Corp [log in to unmask] --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------