This is an interesting one can anyone share there DOE of paste selection and printer setup ----- Original Message ----- From: "John Goulet" <[log in to unmask]> To: <[log in to unmask]> Sent: Sunday, November 02, 2008 7:01 PM Subject: Re: [TN] Controlled RH% Versus Screenprinting Results The viscosity of the solder paste also varies greatly with temperature change that is easier to control. I've had to resolve the same issue at other companies and currently resolving it in this building and layout again. Here are some things to consider before spending $500K. 1. Is the Receiving Dock and Incoming area totally sealed off from the SMT area. It is pretty hard to manage temperature and humidity control with 10' doors open many times a day. In one factory we put up a frame and sheet rock walls around the dock and another for the receiving area. Problem gone. 2. Are the air handlers equipped with programmable thermostates. If they aren't and they don't have the dehumidifier options in them then at night they will blow in cool damp air because it is cool enough the air-conditioner will be acting as a fan only. In the current factory we going to do this before summer. Hopefully we'll also separate our SMT area as stated in #1. 3. Try some of the newly released solder pastes. Indium just came out with 6.3 WS tin/lead that is far better than the 6.2. Senju may not be well known in the USA but in an extensive DOE they were the best for all finishes. Senju is the #1 paste overseas. 4. The paste storage and handling in the productin line to prevent the flux from separating is important. A low voume high mix shop may need to buy 5000 gram or less and not the 7000 gram tubes since you can't put them back in the refrigerator. Large beads of paste over 1/2" may be easier for the operator but in higher humidity and temperature the paste on the stencil is going to change for the worse. The paste spec is written for beads up to 3/4" but that is in ideal RH and temp situations. Small factories that weren't designed for this industry are prone to the same situation that you have. One large factory had a huge sock like air exhange units that blew in whatever air is outside. In the winter you can have small humidifiers added but in the rainy spring and humid summer you have to relay on using the best paste and very good handling controls. Keep the jar low on the rack or floor since since with air conditining the floor will be at a lower temperature approximately 72F. The temperature in the machine it may reach 78-80 if you didn't add the small fan for the summer months. In this way when the operator adds the paste you'll stay in the middle of the control range. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------