We think Solidus/liquidus of Pb/5Sn/2.5Ag is 287/296C So notionally about 16C higher than 80Au/Sn at 280C. I say notionally, as if you review the phase diagram of Au/Sn you will see it is pretty steep on the Au side ramping rapidly up to the MP of Au. So small changes in composition - from taking Au from soldered surface for example - can quickly send you up that side. Hence the difficulty on rework. IN practice both are reflowed around the same temperatures 330-350C. This is because in furnace soldering with a reducing atmosphere you need to be at the high end to get any reduction, and if you are using flux you need to be at the low end to avoid completely killing the flux. In a vacuum oven you just need a long time and the lower the peak the longer. If surfaces are not solderable then pulling a vacuum won't change that. Usually both alloys wet in place with not much spread, however Au/Sn will spread handily if you get it into the high end temp sweet spot. 925Pb/5Sn/2.5Ag is probably one of the most widely used die attach alloys in conventional component assembly. The usual wisdom on soft solders is that they aren't very strong, so the more ductile the alloy the less likely it is to break. This conventional wisdom doesn't really apply to Au/Sn as it is more like a braze with tensile and sheer about 8x 10x lead alloys. It is used where high temp with stand and high temp strength is required (also it has excellent corrosion resistance). Soldering gold surfaces without reducing atmosphere or flux is possible with Au/Sn as no surfaces are oxidised/tarnished. High leads can be used instead of Au/Sn and are clearly much less expensive, but non gold surfaces do tarnish and a reducing atmosphere/flux then has to be considered. Regards Mike Fenner Indium Corporation T: + 44 1908 580 400 M: + 44 7810 526 317 F: + 44 1908 580 411 E: [log in to unmask] W: www.indium.com Pb-free: www.Pb-Free.com --------------------- Indium Corporation Incorporated in New York, USA Registered office: (Not for correspondence) 77-97 Harpur Street, Bedford , UK Registered number: fc16473 -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Creswick, Steven Sent: Thursday, October 09, 2008 8:31 PM To: [log in to unmask] Subject: Re: [TN] Need soldering advice ASAP No II Inge, I'm thinking of greater power cycle endurance for the Pb'ed version as opposed to the super 'hard' Au/Sn. To the best of my knowledge many power FETs are still attached with the high Pb solders to provide some ductility in the joint between the die and copper slug. Si to alumina would present less CTE delta so would be more forgiving for either 'solder' With the Pb'ed version you could possibly go to a Pd/Ag metallization, etc. Subject to your reliability constraints, thereby reducing substrate costs - maybe. Cheaper since no gold would be involved in the solder. Steve -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Inge Sent: Thursday, October 09, 2008 3:09 PM To: [log in to unmask] Subject: Re: [TN] Need soldering advice ASAP No II Right, they did not say that the solder liq is 400C, but that the max chip temp is 400C. That makes sence. Question is what makes this formulae better than AuSn? Do you have any idea? Better wetting or what? Cheaper, but better? Inge ----- Original Message ----- From: "Creswick, Steven" <[log in to unmask]> To: "TechNet E-Mail Forum" <[log in to unmask]>; "Inge" <[log in to unmask]> Sent: Thursday, October 09, 2008 11:51 AM Subject: RE: [TN] Need soldering advice ASAP No II Inge, I could be wrong but I thought that 92.5Pb/5Sn/2.5 Ag was 296°C Liq/289°C Solidus. Assuming ~350°C peak, you ARE really pushing it too far for the seal ring.... If you were using 90Pb/10Sn [302/275], or 95Pb/5 Sn [312/308], I don't see that much difference. Apparently, you are not using 90/10 or 95/5 ?? Steve :-) -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Inge Sent: Thursday, October 09, 2008 1:56 PM To: [log in to unmask] Subject: Re: [TN] Need soldering advice ASAP No II I got an advice from IXYS's support. They recommend quite another solder for their large power MOSFET 's : 92.5Pb/5Sn/2.5Ag. Has anyone of you used it? Will increase the peak temperature from our today's +300C to +400C. They ought to know. But that will melt the sealframe of the package, because it's soldered with AuSn. /Inge ----- Original Message ----- From: "Inge" <[log in to unmask]> To: <[log in to unmask]> Sent: Thursday, October 09, 2008 10:41 AM Subject: Re: [TN] Need soldering advice ASAP No II > Thanks for the support of the linearing idea. I had a feeling that this > could help. > You make me think of placeing the connector on the boards before HASL. > Hmmm...what will happen in the wave soldering of the boards later? > > You started the machinery in my old, gaggy brain....what about applying a > solder mask right over? Is it realistic with that fine pitch? Will the > solder ignore the solder mask and bridge? > > /Inge > > > ----- Original Message ----- > From: "Thayer, Wayne" <[log in to unmask]> > To: "TechNet E-Mail Forum" <[log in to unmask]>; "Inge" > <[log in to unmask]> > Sent: Thursday, October 09, 2008 10:19 AM > Subject: RE: [TN] Need soldering advice ASAP No II > > > Killing the protrusion should linearly improve the process. If you have > cut them to negligible protrusion and still have trouble, then you are > stuck with flux/temperature/time games, or some kind of hot air blow-off > like out of the HASL machine. > > Wayne > > -----Original Message----- > From: TechNet [mailto:[log in to unmask]] On Behalf Of Inge > Sent: Thursday, October 09, 2008 12:31 PM > To: [log in to unmask] > Subject: Re: [TN] Need soldering advice ASAP No II > > Also need advice concerning soldering of a 120 pin, three row, right > angle, through hole edge connector. The pitch is 1 mm, and the through > hole copper collar is such, that the space between them is just a > fraction of a millimeter. We tried to use our selective soldering > machine, but whatever we do, the SnPb overbridges all the pins! I'm not > surprised, because the solder surface tension will not allow the solder > to withdraw pin by pin. > However, such connectors are made and sold plenty of, so they must be > solderable, question is with what. The selective soldering machine's > 'wave pot' is 10 mm across and the minimum wave top is 3 mm. Does it > help to cut the pins so that they are even with the board ? Today, the > pins protrude > 0.3 mms . Anyone who knows nothing? > /Inge > PS. Will send a photo to Dr Gregory. > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 To > unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or > (re-start) delivery of Technet send e-mail to [log in to unmask]: SET > Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the > posts: send e-mail to [log in to unmask]: SET Technet Digest Search the > archives of previous posts at: http://listserv.ipc.org/archives Please > visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for > additional information, or contact Keach Sasamori at [log in to unmask] or > 847-615-7100 ext.2815 > ----------------------------------------------------- > > This e-mail and any files transmitted with it may be proprietary and are > intended solely for the use of the individual or entity to whom they are > addressed. If you have received this e-mail in error please notify the > sender. > Please note that any views or opinions presented in this e-mail are solely > those of the author and do not necessarily represent those of ITT > Corporation. The recipient should check this e-mail and any attachments > for the presence of viruses. ITT accepts no liability for any damage > caused by any virus transmitted by this e-mail. > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 > for additional information, or contact Keach Sasamori at [log in to unmask] or > 847-615-7100 ext.2815 > ----------------------------------------------------- > --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- THE INFORMATION CONTAINED IN THIS E-MAIL MESSAGE AND ANY ATTACHMENTS SENT FROM GENTEX CORPORATION IS GENTEX CONFIDENTIAL INFORMATION INTENDED ONLY FOR THE PERSONAL USE OF THE INDIVIDUAL OR ENTITY NAMED ABOVE. If you are not the intended recipient, you are hereby notified that any review, distribution, or copying of this communication is strictly prohibited. If you have received this communication in error, please immediately notify the sender by return e-mail, and delete this e-mail message and any attachments from your computer. [gntx v.1] --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- ***This email, its content, and any files transmitted with it, are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient, please contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination, or other use of, or taking of any action in reliance upon this information by persons or entities other than the intended recipient is prohibited. Messages sent via this medium may be subjected to delays, non-delivery, and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. Indium Corporation does not accept responsibility for changes made to this email after is was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.*** --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------