----------------------------------------------------- Hi Paymon, The root cause is ENIG 'Black Pad.' In order to protect the electroless Ni from the immersion Au plating bath, P is codeposited. As more and more Ni is dissolved during numerous soldering processes more P is left behind weakening the interfacial structure--the more P, te weaker the interface. Werner -----Original Message----- From: Paymon Sani <[log in to unmask]> To: [log in to unmask] Sent: Thu, 9 Oct 2008 9:57 am Subject: [TN] PCB pad non-wetting issues Hello All, We are experiencing a pad non-wetting issue for the though-hole component pads ONLY! The PCB goes through few heat cycles with top and bottom side assembly during at SMT process and then through-hole assembly at wave process. The problem is found at Wave process. The Pb solder does not wet to the through-hole component pads on the solder side only! An SEM/EDS evaluation revealed high concentration of P in the Nickel and Nickel/Tin intermetalic layer of 11% to 21%. I would like to ask anyone if they have experienced a similar defect in the past. What is the Root Cause? Thank you in advance, Paymon --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------