Victor, There are two types of solder balls. Solder beads and Solder fines. Solder beads that form on the side of chip capacitors not on the pad, but on the FR4 or substrate. This is usually do to paste that get pushed away from the pad under the component or somehow escapes from the pad. Solder fines are much smaller and in my case are around the fillet in the grove between the pad and the FR4 and also on the surface of the fillet. Solder fines are also found on the FR4 away from the components. Leif Erik Laerum Quality Assurance Manager Texas Memory Systems [log in to unmask] Tel: (713) 266-3200 x468 www.texmemsys.com Victor Hernandez wrote: > Can someone clarify the words "and fines" > > -----Original Message----- > From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo > Sent: Friday, August 01, 2008 8:29 AM > To: [log in to unmask] > Subject: Re: [TN] Solder Paste with craters. > > As for ag , you want differant size to increase inter particle contact. > Both size and shape should be in a controlrd range by vender. > -------------------------- > Sent using BlackBerry > > > ----- Original Message ----- > From: TechNet <[log in to unmask]> > To: [log in to unmask] <[log in to unmask]> > Sent: Fri Aug 01 08:07:12 2008 > Subject: Re: [TN] Solder Paste with craters. > > Paul > > You have described a condition that could cause what Leif is seeing. I > think > you have identified the cause of the print anomaly. Adding moisture and > glycol to the print mix could certainly cause paste failure and fines as > well. > > On the subject of type 6 paste; using it for printing in a mix with > standard > parts (0402 passives and .8mm BGA) to accommodate use of fine pitch > flips > and passive arrays? Do you step the stencil? > > We are using type 5 and 6 in dispensers, type 4 for printing parts with > pitches below 0.5 mm. My experience matches Richards (Not with regard to > the > percent metal). The print process window is wider but over all material > performance requires tighter controls and more sophisticated stencil > design. > His brilliant post describing those controls is a prerequisite for > success. > > Want to see a bean counter go crazy? Take him on a shop tour while he > can > observe the air conditioner or room heater battle the humidification > system. > > John, Mike, anyone; care to discuss the relationship of metal powder to > thixotropy? When we specify solder paste % metal by weight, need we > consider > the density of the powder? Increasing the metal by weight to for the > correct > flux by volume to assure desired rheology and thixotropy? > > Is there a standard value for the density of solder powder by type? > > We are working with silver powder in conductive polymers. We find it to > be > variable. But, the powder grain size is not at well controlled as solder > paste spheres. > > Isn't this a cool forum?! > > Guy > > -----Original Message----- > From: TechNet [mailto:[log in to unmask]] On Behalf Of Paul Edwards > Sent: Thursday, July 31, 2008 8:37 PM > To: [log in to unmask] > Subject: Re: [TN] Solder Paste with craters. > > Richard, > > We have been using Type 5 for 2 years with no problems... > Also used type 6 and 6+ without the issues Leif has been having... > Difference is shorter shelf life, more abrupt change when the solder > paste > reaches end of life BUT you can get more solder down on finer > features... > > The solder paste cratering I have seen was from SAC type 4 W/S paste > that > was exposed to moisture and glycol... What occurred was the during paste > printing an air bubble was deposited in the paste or on the > paste...After a > few minutes the bubble would rise to the surface or if on the surface, > would > just burst leaving a small rounded crater in the top of the paste... > > We went back to alcohol for stencil cleaning and opened up a new solder > paste jar and the problem went away... > > Paul Edwards > Surface Art Engineering > > > -----Original Message----- > From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D. > Sent: Thursday, July 31, 2008 2:23 PM > To: [log in to unmask] > Subject: Re: [TN] Solder Paste with craters. > > Hi, Leif > Thanks for your response earlier. It looks like you have a good handle > on > the paste handling, etc. > I was going to ask why a type 5 paste was being used. I have a tough > time > with a type 4, and generally speaking the industry uses a type 3. > With a type 5, you have an order of magnitude more fines, and they are > much > smaller. Because this effectively raises the true metal content above > 94%, > there is actually a little less flux, which I think is a good thing. > But a type 5 is much tougher to control from a printing standpoint. The > fines, being smaller, separate more easily from the agglomeration of the > printed mass, and thus there are more issues with stray fines, and with > small solder balls spitting away in large flat areas, such as under cap > terminations and belly pads, etc. > So the first question is whether you need a type 5 in order to print > through > some very small apertures, such as on flip chips, etc. > If not, try going to a type 4 or 3, and this may help with the stray > fines. > > -----Original Message----- > From: TechNet [mailto:[log in to unmask]] On Behalf Of Leif Erik Laerum > Sent: Thursday, July 31, 2008 2:46 PM > To: [log in to unmask] > Subject: Re: [TN] Solder Paste with craters. > > Interesting feedback. > > The stencil is indeed 6 mil thick. > > The resistor pack pads are 22 x 10 mil and have 20 mil pitch. The > smallest > BGA pads are 20 mil and have 30 mil pitch. > > Is it the case that type 5 has a higher flux percentage than the type 3. > > If so that could explain some of our findings. > > Leif Erik Laerum > Quality Assurance Manager > Texas Memory Systems > [log in to unmask] > Tel: (713) 266-3200 x468 > www.texmemsys.com > > > > Guy Ramsey wrote: > >> Smallest pads under 1 mm BGA + 6 (60 mil??)laser cut stencil + type 5 >> paste = me confused. >> >> This would be, in my opinion, a recipe for hot slump and solder fines. >> > > >> A design with components and features like you describe should be fine >> > > >> with type 3 paste. Let's talk about those capacitor and resistor >> networks. What is their pitch and land pattern dimension? Smaller than >> > > >> the BGA? A lot smaller? Okay maybe type 4 paste and a 4 or 5 mil >> > stencil. > >> Guy >> >> -----Original Message----- >> From: TechNet [mailto:[log in to unmask]] On Behalf Of Leif Erik Laerum >> Sent: Thursday, July 31, 2008 11:34 AM >> To: [log in to unmask] >> Subject: Re: [TN] Solder Paste with craters. >> >> Paul et al, >> >> The bubbles are more prevalent on the smallest apertures such as 1 mm >> BGA pads and the resistor/capacitor pack pads. >> The temperature in the production area is between 68F and 75F. >> Humidity is relatively steady at 40%. (We are in Houston....) >> >> If anyone has any suggestions how to test the screens for cleanliness >> that would be great. That is a part of our process we do not control. >> We have a stencil cleaner, but we can only visually see if they are >> really getting clean. We also bought some stencil cleaner for manually >> > > >> wiping down a screen, but it actually makes the screens "greasy". We >> > stopped using it. > >> Ours stencils are the standard 60 mil laser cut. We do use a metal >> > squeegee. > >> >> >> Leif Erik Laerum >> Quality Assurance Manager >> Texas Memory Systems >> [log in to unmask] >> Tel: (713) 266-3200 x468 >> www.texmemsys.com >> >> >> >> Paul Edwards wrote: >> >> >>> Leif, >>> >>> I just have 2 questions... >>> >>> What size apertures do these bubbles occur on and is there a >>> particular aperture orientation in which they are prevalent? >>> >>> What is the humidity and temperature of the environment for the paste >>> > > >>> prior to putting it on the stencil>> >>> >>> Have seen something similar in certain kinds of SAC W/S pastes that >>> have been exposed to too much moisture and certain stencil cleaning >>> compounds...The saponifier was making soap bubbles when rolling in >>> the paste... >>> >>> Paul >>> Paul Edwards >>> Surface Art Engineering >>> >>> >>> >>> >>> >>> >>> -----Original Message----- >>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Leif Erik Laerum >>> Sent: Wednesday, July 30, 2008 1:56 PM >>> To: [log in to unmask] >>> Subject: Re: [TN] Solder Paste with craters. >>> >>> Thank you everyone for contributing. Especially you, Richard. >>> >>> First of all these are NOT via in cap boards and we are using FR4. >>> Been there done that.... >>> >>> Most of the items brought up by Richard we do have established >>> processes for. These are according to the recommendations of the >>> solder vendor, but if others feel differently, please chime in. >>> We log the solder used for each batch and the Date of Manufacture >>> for this. We typically do not accept a batch of solder that is older >>> > > >>> than 3 mts. This is so that we do not end up with too much out of >>> date solder at the end. >>> >>> - Solder is brought out of the fridge minimum 12 hours before use. >>> - We set a time limit that solder must can be stored out of the >>> fridge a maximum of 3 mts. Practically this ends up around 1 month >>> > max. > >>> - We do reuse solder that has been on the screen for up to two weeks. >>> Then we throw it out. >>> - We never put solder back in the fridge. >>> - We are evaluating new suppliers of solder at the moment. We have >>> not audited the currents supplier, but that is a good idea. We always >>> > > >>> get the solder couriered locally and in a cool container so I do not >>> have any evidence that would lead me to put this on the solder >>> vendor, but..... >>> - As our process works boards sit no longer than 1 hour with solder. >>> Usually much shorter than that. >>> - We are using Type 5 solder actually. >>> - All misprints go though the wash before it is reprinted. >>> - We use a DEK 248 that is not as automatic as I would like and some >>> of the issues we see are due to this repeatability problem, but from >>> the data I have gathered, this is not the cause of the solder fines >>> and craters. >>> - A Solder AOI would be nice. We do not have one of these (yet???) >>> - There could be an issue with too much solder. We are going to >>> reduce apertures some. There is some evidence of excessive solder. >>> - I am going to experiment with slowing down the print separation >>> > speed. > >>> Good point. >>> >>> Thx. >>> >>> Leif Erik Laerum >>> Quality Assurance Manager >>> Texas Memory Systems >>> [log in to unmask] >>> Tel: (713) 266-3200 x468 >>> www.texmemsys.com <http://www.texmemsys.com> >>> >>> >>> >>> Inge wrote: >>> >>> >>>> Hi Leif, you've just listened to His Master's Voice. >>>> You should take off your cap, when you speak to Richard Stadem. >>>> Impressive! I begin to feel that there are two exceptional stars at >>>> > TN. > >>>> Steve...we already knew >>>> Richard...a supernova >>>> >>>> Inge >>>> >>>> Gah...my example was not very clever...a supernova is bright just >>>> for a short time...hmmm...a red giant then? hmmm...or a white >>>> dwarf...hm...none of them very striking....hmm....shining like >>>> Betelgeuse...hmm.....maybe Master Whittaker can give a hand? >>>> >>>> >>>> ----- Original Message ----- From: "Stadem, Richard D." >>>> <[log in to unmask]> >>>> To: <[log in to unmask]> >>>> Sent: Wednesday, July 30, 2008 6:53 AM >>>> Subject: Re: [TN] Solder Paste with craters. >>>> >>>> >>>> Hi, Leif >>>> Send your pictures to [log in to unmask] >>>> >>>> Can you tell me what solder paste it is you are using? How was it >>>> qualified for use? >>>> >>>> Here are just some of the questions you need to ask yourself in >>>> order to determine why you have an issue with solder fines: >>>> Do you have a good documented solder paste handling procedure? How >>>> is the paste handled, from vendor or distributor to your factory? >>>> When was the last time you stopped in at the distributor to verify >>>> their stock is being rotated and is kept refrigerated immediately >>>> upon receipt from the factory? How often do they turn the packages >>>> upside down to prevent flux separation? Are they a certified >>>> distributor who will pass on to you a lot recall notice from your >>>> solder paste vendor if there is a known bad lot? >>>> How long is the paste allowed to sit out on the stencil and how many >>>> > > >>>> times can a line of paste on the stencil be sheared (printed back >>>> and >>>> forth) before it is removed and replenished with fresh paste? Are >>>> the operators allowed to scrape up the unused paste on the stencil >>>> and re-deposit it into a jar for re-use later? Is the jar or tube of >>>> > > >>>> solder paste, once removed from refrigeration, allowed to set for >>>> two to four hours (depending on paste vendor and paste type) to >>>> reach room temperature prior to printing? Once removed from the >>>> refrigerator, is unused solder paste allowed to be put back in the >>>> refrigerator? Are you using Type 4 paste or Type 3? How good is the >>>> printer setup, ie, the repeatability of the registration of the >>>> stencil to the PWB? Are you performing some type of aperture >>>> reduction on all pads in general and at least a 50% reduction on >>>> large belly pads to prevent solder fines from being printed onto the >>>> > > >>>> board? If a board is misprinted, does the operator know better than >>>> to simply wipe off the board (embedding the paste into every space >>>> between the edges of the pads and the soldermask, into every small >>>> via, into every through hole, etc.) but is there a documented >>>> procedure detailing how the misprinted board is to be cleaned to >>>> prevent this? How is the solder paste packaged, jar or tube? (Tubes >>>> prevent a much larger volume of paste from being exposed to air and >>>> humidity, and also help prevent re-use of solder paste that has been >>>> > > >>>> out for awhile). Do you perform a good solder paste print inspection >>>> > > >>>> using a 3d AOI or some other type of automated inspection, and do >>>> you use the data from this inspection process to detect (real-time) >>>> >>>> >> paste defect trends and react to them with corrective actions? >> >> >>>> Sorry to ask so many questions, but all of these can contribute to >>>> fines, and there are many more factors that can cause them. >>>> >>>> >>>> >>>> -----Original Message----- >>>> From: TechNet [mailto:[log in to unmask]] On Behalf Of Leif Erik Laerum >>>> Sent: Wednesday, July 30, 2008 8:29 AM >>>> To: [log in to unmask] >>>> Subject: [TN] Solder Paste with craters. >>>> >>>> Technetters, >>>> >>>> We are having an issue with solder fines on our lead free boards. We >>>> > > >>>> are using SAC305 WS and no nitrogen. I noticed that our boards have >>>> craters in the paste on the pads after being printed. Not all pads >>>> are deposited this way, but maybe 25%. These craters have an air >>>> bubble in them. The bubbles usually burst before the boards goes >>>> into the P&P, but the crater stays. The screening process is exactly >>>> > > >>>> the same for leaded and unleaded paste. The leaded paste does not >>>> behave this way. Could these craters be a symptom of the cause of >>>> the solder fines? Anyone have any experience with this? >>>> >>>> How do I go about posting pictures to stevezeva.homestead.com?. >>>> >>>> >>>> -- >>>> Leif Erik Laerum >>>> Quality Assurance Manager >>>> Texas Memory Systems >>>> [log in to unmask] >>>> Tel: (713) 266-3200 x468 >>>> www.texmemsys.com <http://www.texmemsys.com> >>>> >>>> > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with following text > in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: > http://listserv.ipc.org/archives > Please visit IPC web site > http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional > information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 > ext.2815 > ----------------------------------------------------- > > --------------------------------------------------------------------- > This transmission (including any attachments) may contain confidential > information, privileged material (including material protected by the > solicitor-client or other applicable privileges), or constitute > non-public information. Any use of this information by anyone other than > the intended recipient is prohibited. If you have received this > transmission in error, please immediately reply to the sender and delete > this information from your system. Use, dissemination, distribution, or > reproduction of this transmission by unintended recipients is not > authorized and may be unlawful. > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with following text > in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: > http://listserv.ipc.org/archives > Please visit IPC web site > http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional > information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 > ext.2815 > ----------------------------------------------------- > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: http://listserv.ipc.org/archives > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 > ----------------------------------------------------- > --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------