Ioan, If you strongly believe it is mechanical stress from removing assemblies from the array, try removing them without the stress of bending. If the fab shop scored them well enough you should be able to taken a razor knife along the v-scored area repeated times until the rails just about fall off by themselves. If you can remove them without mechanical stress, and see no opens at the solder joints, then you just might have isolated the cause (being of course mechanical stress); however, if you see opens...well then look at your solder process again. Franklin -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea Sent: Friday, July 18, 2008 2:18 PM To: [log in to unmask] Subject: Re: [TN] Mechanical damage to BGA Vladimir, You have some good points, just like Victor. The process is leaded and I have no idea when the damage occurs. We've only built 20 pieces, inspected them under the microscope and only realized there is a problem at test. Under limited investigative resources, I can only say that everything makes me believe the soldering recipe is good enough to create proper joints and that I suspect mechanical action to be the cause. Therefore I can only rely on this forum's expertise and try to figure out whether this is really an over the edge design, or rather something normal. If the design is too much, how can it be improved? If the design is regular stuff, I will put more effort in controlling depanelizing and handling. Thanks, Ioan -----Message d'origine----- De : Igoshev, Vladimir [mailto:[log in to unmask]] Envoyé : July 18, 2008 3:01 PM À : TechNet E-Mail Forum; Ioan Tempea Objet : RE: [TN] Mechanical damage to BGA Hi Ioan, You didn't specify the type of the joints/process (Pb-free?) and when the joints fail? Is it right after the SMT and if that is the case, then what is the cooling rate for the assembly. Larger pads could help, of cause (almost any larger thing can carry a larger load - I'm curious are there going to be any Friday comments on that statement? :-)) Regards, Vladimir -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea Sent: Friday, July 18, 2008 2:48 PM To: [log in to unmask] Subject: [TN] Mechanical damage to BGA Dear Technos, I have this BGA that gives me a headache. In many instances the boards do not pass test, we press on the BGA and they start working; a classic... The problem solder joints are always on the same side of the component and on the outer row; needless to say, we have a V-groove line that is manually cracked. So the cause is most likely mechanical stress that causes the pads to detach from the PCB. After prying off some BGAs we see the soldering is good, all the pads come off the board and stay solidly attached to the balls. The specifics of this board are a bit special and I would need your opinion on what to improve in the design in order to eliminate the propensity to damage. PCB is 18.55x28.65mm, FR4, 0.55mm [0.021"] thick The BGA is 17x17mm, 1mm pitch, 0.65mm balls assembled on 0.25mm circular pads. In the troubled zone the pads are connected to 0.050mm traces. My opinion is that the board flexes very easily and even if we fix the depanelization (I will modify the panel) all the subsequent handling, including the integration of this module, puts the joints at high risk. I think the pads are too small so they do not have sufficient adhesive force to stay put on the PCB. On top of it, the traces are so minute, so the slightest stress will be destructive. Would increasing the pad size help? Is this construction (thin PCB + superfine traces) viable? Could the CTE mismatch be strong enough to cause the damage, instead of the mechanical stress from bending the board? Thank you, Ioan --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------