Pete, A good XRF and a calibrated set of thickness standards will tell you if you have ENIG within thickness specs for this finish. Also dab some solder paste on board pads, shoot it through a normal reflow and inspect the results: 1) Does the solder wet out the pad nicely? 2) Can you flick off the re-solidified solder with your fingernail (obviously a bad sign)? 3) Look at the x-section of the joint. Is there evidence of a continuous tin/nickel intermetallic layer? Bev RIM -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of R Sedlak Sent: Monday, July 21, 2008 6:39 PM To: [log in to unmask] Subject: Re: [TN] looking for ENiG photos Pete: I come in late to this discussion, and may have missed salient points. Do you suspect the deposit is immersion gold over Copper, with the EN missing, or do you suspect electrolytic gold over electrolytic Nickel? If you suspect immersion Gold over Copper (no EN) simple baking should tell the tale, causing the intermetallic to form. Rudy Sedlak --- On Mon, 7/21/08, Pete Houwen <[log in to unmask]> wrote: > From: Pete Houwen <[log in to unmask]> > Subject: Re: [TN] looking for ENiG photos > To: [log in to unmask] > Date: Monday, July 21, 2008, 12:54 PM > Inge, > > Very good point! > > background: The purchasing agent who is driving this has a > bonus riding on > reducing PCB fabrication costs by $125K this year - with no > adjustment for oil > or copper costs. So if she saves $125K and manufacturing > costs go up $500K, > she gets a bonus. Not to mention their longstanding > tradition of being penny > wise and pound foolish. > > Wit that, what are my chances of getting time or funding > for a "really good > qualification"? Supposedly the D&B was done - I > don't get that info. Someone > from our Shanghai R&D group visited the plant - but > he's not a PCB guy. I > already know that their stated abilities don't meet our > specs. Manufacturing > doesn't want this. We've just spent months getting > our processes somewhat > reliable, adding junk plating to it isn't going to > help. > > But there's that bonus. So I've got these > pictures.... I don't want to lie, or > exaggerate (much), but if I could find something > comparative to scare the > bean counters...... they just don't get the value of > paying for quality up front. > > I keep a curled up tie and round glasses in my office to > wear during projects > like this....... > > Pete > > --------------------------------------------------- > Technet Mail List provided as a service by IPC using > LISTSERV 15.0 > To unsubscribe, send a message to [log in to unmask] with > following text in > the BODY (NOT the subject field): SIGNOFF Technet > To temporarily halt or (re-start) delivery of Technet send > e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) > To receive ONE mailing per day of all the posts: send > e-mail to [log in to unmask]: SET Technet Digest > Search the archives of previous posts at: > http://listserv.ipc.org/archives > Please visit IPC web site > http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for > additional information, or contact Keach Sasamori at > [log in to unmask] or 847-615-7100 ext.2815 > ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------