Pete, I may be wrong, but I claim that there is no ENIG reference picture or pictures. ENIG can have many faces, large 'grain' clusters, small clusters, bright appearance and dull, typical gold colored and more like copper color, hard surface and rather soft one, super flat and like Rocky Mountains seen in a SEM....it all depends (TM). There are some traps also...you can study a ENIG board sample in a SEM, look hard on it with a LOM, do EDAX and other advanced investigations and find everything looking 'good', while, at the same time, the sample is impossible to solder at. And vice versa. For a serious qualification, I recommend some of the programs used by anyone with this forum, George Wenger, Dave Hillman, Richard Stadem or similar experienced guy. Myself, I could send lots of 'ENIG pictures' but I'm afraid these wouldn't be enough for a qualification. If you really mean to make a good qualification job, you'd better sit down and mail to any of the mentioned gurkas...sorry..gurus. Inge PS. If noone supports you, I'll send something offline to you, but later when I'm at my office. ----- Original Message ----- From: "Pete Houwen" <[log in to unmask]> To: <[log in to unmask]> Sent: Monday, July 21, 2008 6:58 AM Subject: [TN] looking for ENiG photos Our purchasing group is trying to qualify a new low cost PCB vendor, and I have some reservations. I have been examining their sample boards, and while one oif them shows a normal ENiG grain under 800x magnification, the other is flat and dull. I believe it might be just gold plating. It's hard to tell from the cross sectons they sent (those display their own set of concerns). I'm trying to find some images to compare these, but I'm having no luck. Does anyone know of a good site where I might find some ENiG and Gold images? Thanks, Pete --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------