Joyce, Representative measurements have been very similar to those shown below... 70% iron 18% chromium 11% nickel No zinc was found in the material analysis. Leland -----Original Message----- From: Joyce Koo [mailto:[log in to unmask]] Sent: Tuesday, May 13, 2008 2:26 PM To: [log in to unmask]; Leland Woodall Subject: Re: [TN] Stainless Steel Contamination Question Are you sure it is steel, not zn? -------------------------- Sent using BlackBerry ----- Original Message ----- From: TechNet <[log in to unmask]> To: [log in to unmask] <[log in to unmask]> Sent: Tue May 13 10:21:57 2008 Subject: Re: [TN] Stainless Steel Contamination Question Hi John, The material we're finding is loose and in contact with and intermittently bridging pins on our ICs. We apply conformal coating to our products, and of course, when the compound hardens, it pulls even tighter to the leads and causes a failure. I'll verify that the air handling and reflow oven systems have indeed been checked. Thanks for your reply! Leland -----Original Message----- From: John Burke [mailto:[log in to unmask]] Sent: Tuesday, May 13, 2008 10:16 AM To: 'TechNet E-Mail Forum'; Leland Woodall Subject: RE: [TN] Stainless Steel Contamination Question On top............... How are they connected or are they loose? Have you checked any overhead air handling equipment? Looked at the filtering in freflow ststems etc? JOhn John Burke (408) 515 4992 -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall Sent: Tuesday, May 13, 2008 6:47 AM To: [log in to unmask] Subject: [TN] Stainless Steel Contamination Question Importance: High Hi Everyone, We've had a problem lately with fine strands of stainless steel wire being found on top of some of our .5 mm pitch ICs. This has caused both internal and external issues, and we've yet to identify the source. It's definitely formed wire, with a thickness ranging from 7 to 10 microns, and up to 3 mm in length. Our automated optical inspection stations can only reliably detect widths of 12 to 15 microns. I've checked the internet in an attempt to find common applications of this wire. I've found two, and they were for ultra-fine filters and stencil screen mesh. We've investigated (I think) all of our machinery that would utilize filters this small and have found no such usage. I've also checked every stencil in our plant, and all of our mesh material is some type of a plastic compound. Do you have any idea where this stainless steel might be coming from? Any suggestions would be sincerely appreciated! Thanks, Leland --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------------------------- This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful. --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------