Hi Ryan, I reviewed the pictures you sent and I would describe this condition as a circumferential barrel crack. The crack presents itself and a metal fatigue type crack in that it starts at a glass fiber and proceeds around copper crystals at an angle. The crack is closed at ambient suggesting the material has not been significantly degraded (it is still elastic) and not expressing a mechanical "hysteresis" as it were. The black area in the PTH you mentioned is a slight copper etch in the middle of the barrel. I notice that you can see the black area through the mounting compound at the back of the hole and as a cross sectional view on the edge of the PTH. The copper under the corroded area appears well plated. I expect the corroded areas in the central zone of the barrel to focus stress and be a site for crack initiation. I would guess the board dried with a slightly corrosive liquid in the PTH. As the liquid evaporated the solution became more concentrated and corroded the copper in the central zone. Possibly a combination of poor rinsing (or contaminated rinse water), slow drying or a humid environment contributed to this condition. All things considered the drilling and hole preparation is better than most. If the copper is about 20 um then the roughness is less than 2 um which is good. I have seen robust vias with worse hole prep. Drilling and hole preparation is not a concern in my book. The black triangle in the dielectric is associated with the copper crack but probably not the cause of the crack. I frequently see the glass and the resin near a copper crack disturbed. I think the epoxy and glass near the copper crack is fractured and pieces can fall out during microsectioning. This is not a cause of failure but an indicator that there is damage in the area. I would confirm copper elongation and ductility are within acceptable ranges. Also confirm the temperature used in assembly are correct for the application (tin-lead vs. lead-free), and assure the material is robust in that application. Sincerely, Paul Reid Program Coordinator PWB Interconnect Solutions Inc. 235 Stafford Rd., West, Unit 103 Nepean, Ontario Canada, K2H 9C1 613 596 4244 ext. 229 Skype paul_reid_pwb [log in to unmask] <mailto:[log in to unmask]> -----Original Message----- From: TechNet [mailto:[log in to unmask]] On Behalf Of Ryan Grant Sent: Tuesday, April 22, 2008 1:43 PM To: [log in to unmask] Subject: [TN] Via barrel cracks Hi Technetters, I have a case of via barrel cracks (E crack) and I would like to know possible causes. The crack is circumferential and occurs at the center of the via. The hole appears smooth, i.e., no glass nodules or tearout and there is neither positive nor negative etchback. Of course there is some wicking, but only about 25um max. The copper thickness is 20um at the crack and roughly 35-40um at the knee. Although, at the initiation point of the crack, the copper thickness is only 10um, but that could be due to stretching and subsequent thinning of the copper. Around the periphery of the crack are micro-voids in the resin about 30um. It is triangular shaped, so I can't tell if it is resin recession or a laminate crack. In other words, this via pretty much looks normal, except for one thing, which might be an artifact of stretching and cracking of the via. For a span of about 60um on the vertical of the via, at the crack, there is a roughness that slightly reduces the copper thickness. The surface of the copper at this point appears both rough and black in color. This board has seen two reflows and a hot functional test before final failure. The board shop's initial response was speculation of the OSP soft etch attacking the copper, but this particular via has solder mask plugging both sides of the via; therefore chemicals after solder mask cure can not get into the via. In case it matters, at one time, we have had occurrences of this board shop "re-working" panels after copper plating by placing the panel in a tank of etchant, then re-running the board through copper plating. (They do panel plating). I'm a little suspicious of their FA, so I would like some independent opinions and places for me to dig into. Thanks for any help, Ryan --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 ----------------------------------------------------- --------------------------------------------------- Technet Mail List provided as a service by IPC using LISTSERV 15.0 To unsubscribe, send a message to [log in to unmask] with following text in the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest Search the archives of previous posts at: http://listserv.ipc.org/archives Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 -----------------------------------------------------